5.2
Impact Factor
Generic selectors
Exact matches only
Search in title
Search in content
Post Type Selectors
Search in posts
Search in pages
Filter by Categories
Corrigendum
Current Issue
Editorial
Erratum
Full Length Article
Full lenth article
Letter to Editor
Original Article
Research article
Retraction
Retraction notice
Review
Review Article
SPECIAL ISSUE: ENVIRONMENTAL CHEMISTRY
5.3
Impact Factor
Generic selectors
Exact matches only
Search in title
Search in content
Post Type Selectors
Search in posts
Search in pages
Filter by Categories
Corrigendum
Current Issue
Editorial
Erratum
Full Length Article
Full lenth article
Letter to Editor
Original Article
Research article
Retraction
Retraction notice
Review
Review Article
SPECIAL ISSUE: ENVIRONMENTAL CHEMISTRY
View/Download PDF
Original Article
2025
:18;
3132025
doi:
10.25259/AJC_313_2025

Translate:

Effects of carbon nanomaterials modified hexaphenoxycyclotriphosphazene on the properties of polymethyl methacrylate

Author affiliations
Shandong Key Laboratory of Eco-Environmental Science for the Yellow River Delta, Shandong University of Aeronautics, Binzhou, Shandong, 256603, China
Article History
Corresponding author(s)

*Corresponding author: E-mail address: wbh3337@163.com (L. Xu)

Article tools · PDF & citations

Abstract

Oxidized carbon nanotubes (CNTs), fullerene (C60), and graphene oxide (GO) prepared via the Hummers method were reacted with hexaphenoxycyclotriphosphazene (HPCTP) to form N/P/C ternary flame retardants. Flame-retardant polymethyl methacrylate (PMMA) composites were then prepared via an in situ polymerization method. The results of material performance research showed that C60@HPCTP exhibited the most effective flame-retardant performance‌, evidenced by a 47.4% increase of the limiting oxygen index (LOI) and a 54.0% reduction in the peak heat release rate (pHRR) relative to pure PMMA, while the LOI increases for CNTs@HPCTP and GO@HPCTP were 40.6% and 41.1%, and the pHRR reductions were 43.0% and 48.4%, respectively. Post-combustion residues of the PMMA composites were characterized by scanning electron microscope (SEM) and Raman spectroscopy. The SEM images revealed a continuous, compact char layer formed via the catalytic carbonization effect of HPCTP and the nanofillers (CNTs/GO/C60), which act as a physical barrier to the heat and mass transfer. Raman spectra further confirmed enhanced graphitization (AD/AG ratio reduced by up to 26.2% compared to pure PMMA), indicating improved thermal stability of the char. The synergistic flame-retardant effect in the condensed phase arises from the protective coating generated by phosphorus in HPCTP, the crosslinked network formed by carbon nanomaterials, and the carbonaceous char layer resulting from their co-catalyzed dehydration of PMMA, while in the gas phase, synergistic mechanisms involve the dilution effects of nitrogen as well as the radical quenching effect by phosphorus species and carbon nanomaterials. The synergistic effect of nitrogen, phosphorus, and carbon effectively inhibits the occurrence and development of combustion, and significantly improves the flame retardancy of PMMA.

Keywords

  • Carbon nanomaterial
  • Flame retardant
  • Hexaphenoxycyclotriphosphazene
  • Polymethyl methacrylate
Licence
This is an open-access article distributed under the terms of the Creative Commons Attribution-Non Commercial-Share Alike 4.0 License, which allows others to remix, transform, and build upon the work non-commercially, as long as the author is credited and the new creations are licensed under the identical terms.

1. Introduction

Carbon nanomaterials are widely employed in flame-retardant polymer composites owing to their exceptional fire suppression efficiency [1]. Nevertheless, when implemented as standalone additives at low loading levels, these nanomaterials exhibit suboptimal flammability reduction performance. Conversely, excessive incorporation frequently leads to poor dispersibility within the composite architecture, thereby compromising tensile modulus and other original properties of the composite material [2]. Moreover, the inherent incompatibility between carbon nanomaterials and nonpolar polymer matrices often results in poor interfacial adhesion and phase separation, further limiting homogeneous dispersion. Additionally‌, structural degradation under high-shear processing conditions reduces their aspect ratio and catalytic activity, diminishing their ability to form protective char layers during combustion. These challenges necessitate innovative surface modification strategies to unlock their full potential. Thereby, carbon nanomaterials are compounded with traditional flame retardants to reduce their fraction and form a synergistic system, in which the advantages of different flame retardants are fully utilized, so that the prepared flame-retardant composites have distinguished flame-resistant capabilities, physical properties related to mechanics, and thermal stability simultaneously [3]. According to correlative references, carbon nanomaterials create synergistic effects with multiple traditional flame retardants such as metal (hydrogen) oxides [4,5], nitrogen-based flame retardants [6,7], phosphorus-based flame retardants [8-10], and other nano-flame retardants [11,12]. Among them, phosphorus-based flame suppressants possess the benefit of minimal smoke emission, non-hazardous nature, superior fire resistance, and excellent matrix compatibility, which makes them widely used in flame retardant polymers [13,14].

Hexaphenoxycyclotriphosphazene (HPCTP, C36H30N3O6P3) is a commonly used phosphorus flame retardant, which has significant fire-resistant performance in both condensed and gas phases, considering the presence of nitrogen and phosphorus. Recently, HPCTP has gained broad application as a fire-resistant agent for polymers such as epoxy resins, polycarbonates, and polypropylene [15]. Yuan et al. [16], Seraji et al. [17], and Yan et al. [18] employed HPCTP as a flame retardant for expandable polystyrene (EPS), epoxy resin, and glass fiber-reinforced polyamide 6 (GF/PA6), respectively. It was found that HPCTP could drastically cut down the heat-release rate of polymers and improve their limiting oxygen index (LOI). When HPCTP was broken down by heat, it absorbed heat and formed inert gases like NH₃ and N₂, effectively lowering the concentration of volatile flammable gases and oxygen. During combustion, HPCTP released volatile phosphorus species like PO· and PO2˙, effectively scavenging flammable free radicals in the gaseous phase while generating char layers and impeding the transfer of mass and heat in the condensed phase. While HPCTP demonstrates flame-retardant functionality as a standalone additive, its inherent efficiency limitations typically necessitate loading levels exceeding 10 wt% to achieve targeted flame-retardant efficacy. Such elevated concentrations frequently compromise the inherent properties of the polymer matrix, particularly its mechanical performance. Strategic formulation with complementary flame retardants is therefore recommended to exploit synergistic interactions between different flame-retardant mechanisms, thereby enabling optimized additive dosage while preserving material integrity.

Studies by Shen et al. [19], Lyu et al. [20], and Chen et al. [21] demonstrated that HPCTP exhibited synergistic flame-retardant effects when combined with magnesium hydroxide (MH), diatomite (Dia), and ionic liquid-modified graphene, respectively. These combinations achieved significantly enhanced flame-retardant efficiency compared to single-component systems. Notably, HPCTP also improved the interfacial compatibility between flame retardants and the polymer matrix, which mitigated performance degradation caused by additive agglomeration. The above studies show that HPCTP has a synergistic effect with various types of flame-retardant agents. However, few studies have been conducted on the synergistic effect of HPCTP and carbon nanomaterials. The combination of carbon nanomaterials with HPCTP not only enables the utilization of polar functional groups within HPCTP (e.g., P=O and N-H) to weaken the intermolecular van der Waals forces among carbon nanomaterials, thereby reducing agglomeration and enhancing dispersion stability, but also integrates the flame-retardant mechanisms of carbon, phosphorus, and nitrogen to achieve full-temperature-range synergistic protection from low-temperature radical quenching to high-temperature char layer reinforcement. This collaborative mechanism overcomes the technical bottleneck of temperature limitations associated with conventional phosphorus-based flame retardants while substantially addressing critical gaps in existing research domains.

Polymethyl methacrylate (PMMA), a widely utilized thermoplastic polymer, exhibits exceptional mechanical strength, notable chemical resistance, and outstanding molding capabilities. However, this material demonstrates limited thermal stability with a critically low LOI of 17.3%, which means it can be ignited at a lower oxygen concentration. Its combustion process generates substantial exothermic energy, thereby creating significant safety hazards for both personnel and the surrounding environment [22-24]. Therefore, it cannot be applied to high-temperature environments or places with multiple ignition sources and high fire risk unless its flame retardant performance is improved. In this study, carbon nanotubes (CNTs), graphene oxide (GO), and fullerene (C60) were used to modify HPCTP and form a ternary synergistic system of nitrogen, phosphorus, and carbon. This innovative system orchestrated three complementary flame-retardant mechanisms: the catalytic carbonization and coverage effect of phosphorus, the dilution and inserting effect of nitrogen, as well as the physical barrier and char layer optimization effect of carbon. The synergistic interplay between these mechanisms enhanced the fire suppression efficiency of the flame retardant, thereby enabling a marked reduction in its dosage. In addition, HPCTP improved the dispersion of carbon nanomaterials, enabling the formation of a uniform cross-linked network within the matrix, which enhanced the mechanical properties of PMMA. Compared to conventional carbon nanomaterial-based systems, the strategic implementation of carbon-engineered HPCTP as multifunctional flame retardants demonstrated superior cost-performance efficiency. To investigate the effects of modified HPCTP on the properties of PMMA, thermogravimetric analysis (TGA) was applied to assess the material’s thermal stability, while LOI tests and cone calorimetry were conducted to evaluate its flame-retardant performance. Furthermore, the morphology of combustion residues, combined with X-ray photoelectron spectroscopy (XPS) and Raman spectroscopy, was systematically analyzed to investigate the flame-retardant mechanisms of the composite.

2 Materials and Methods

2.1. Materials

Methyl methacrylate (MMA, AR), polyvinyl alcohol (PVA, AR), azobisisobutyronitrile (AIBN, AR), hexachlorocyclotriphosphazene (HCCP, 98%), multi-walled CNTs (90%), C60 (99.5%), graphite powder (99.95%), tetrahydrofuran (THF, AR), n-Heptane (AR), and sodium hydroxide (NaOH) were purchased from Shanghai McLin Biochemical Technology Co., Ltd. Sodium nitrate (NaNO3, AR) was supplied by Tianjin Kaitong Chemical reagent Co., Ltd. Potassium permanganate (KMnO4, AR) was furnished by Jintan Experimental Factory, Shanghai Institute of Chemical Industry. Potassium persulfate (KPS, 99%), potassium hydroxide (KOH, 95%), hydrogen peroxide (H2O2, 30%), and phenol (AR) were provided by Tianjin Tianli Chemical Reagent Co., Ltd. Sulfuric acid(H2SO4, 98%) was offered by Yantai Yuandong Fine Chemical Co., Ltd.

2.2. Instruments

The architecture of the composites was elucidated through Fourier transform infrared spectroscopy (FTIR) (NICOLET 380, Nicolet Instruments, America). The material’s thermal stability was assessed using a synchronous thermal analyzer (STA449F3, Necchi Instrument Manufacturing Co., Ltd., Germany). The flame-retardant characteristics were evaluated using an oxygen index tester (SH5706A, Guangzhou Xinhe Electronic Equipment Co., Ltd., China) and a cone calorimeter (FTT iCone Classic, Fire Testing Technology Limited, the UK). The structure of the carbon residue following the cone calorimeter test was examined using a scanning electron microscope (SEM) (Hitachi SU8010, Hitachi Limited, Japan). The XPS (Thermo Kalpha, Thermo Fisher Scientific, America) and Raman spectra (LabRAM HR Evolution, HORIBA, France) of the carbon residues were analyzed.

2.3. Preparation of composite materials

2.3.1. Synthesis of HPCTP

A three-necked flask fitted with a condensation reflux apparatus was charged with phenol (22.59 g), sodium hydroxide (9.6 g), and Tetrahydrofuran (THF) (120 mL) solution. The flask was raised to 45°C in a thermostat water bath, and the mixture was stirred continuously for 2 h. Then the reactant was heated to 90°C for azeotropic distillation to remove the water, and the liquid in the flask was cooled down to ambient temperature to generate sodium phenol solution. Next, HCCP (10.43 g) was fully dissolved in THF solution, and the mixture was slowly added to the sodium phenol solution with a constant pressure drip funnel. The mixture was heated to 65°C and stirred continuously for 48 h to ensure the reaction proceeded to completion. The reactant was reduced to room temperature and concentrated by vacuum filtration. Then, it was added to deionized water, and some white precipitate was obtained. To improve the quality of products, the filtration was carried out again, and the crude product of HPCTP was obtained. The crude product was recrystallized with a mixture of THF and n-heptane, and subsequently vacuum-dried at 65°C for 5 h to obtain the white HPCTP powder.

2.3.2. Preparation of HPCTP modified by carbon nanomaterials

For this procedure, 1 g GO (prepared by Hummers method), 4 g HPCTP, and 100 mL THF were added into a beaker and stirred for 2 h after being ultrasonically dispersed for 30 min to make them fully dissolved. The mixture was then transferred to a high-pressure reactor, which was pre-purged with nitrogen gas. The reactor was then transferred to a muffle furnace at 150°C to allow the materials inside to react for 5 h. After filtration, the reaction products were rinsed three times with deionized water, followed by drying in a vacuum oven at 60°C for 12 h to produce the GO-modified HPCTP (GO@HPCTP) powder.

Carbon nanotubes (CNTs) and C60 were first oxidized according to the methods in reference [25] and reference [26], respectively, and then reacted with HPCTP according to the above steps to obtain CNTs modified HPCTP (CNTs@HPCTP) and C60 modified HPCTP (C60@HPCTP).

2.4. Preparation of modified HPCTP/PMMA composites

Precisely measured quantities of GO@HPCTP, C60@HPCTP, and CNTs@HPCTP nanocomposites were subjected to ultrasonic dispersion in deionized water, yielding monodisperse aqueous suspensions with precisely controlled concentration gradients (5 mg/mL and 10 mg/mL). Then, 40 mL aqueous solution with different concentrations was poured into a three-necked flask, and 3 mL Polyvinyl alcohol (PVA) solution with a volume fraction of 5% was added dropwise. The flask was situated in a temperature-controlled water bath at 40°C, while the mixture inside was agitated at a speed of 400 rpm. Then, 12 g Methyl methacrylate (MMA) was poured into the flask, and 0.16 g Azobisisobutyronitrile (AIBN) was added evenly at 50°C, 60°C, and 70°C. When the temperature reached 78°C, the heating was stopped. In the heating process, a magnetic stirrer was used to remove bubbles from the reaction system. When the mixture became glycerol-like, the flask was cooled in an ice bath. When the solution became viscous, it was poured into a mold and then dried in a vacuum drying box at a temperature of 35°C for 12 h to solidify. After curing, the composite material was cooled and demolded at room temperature.

Composites prepared with different concentrations of GO@HPCTP solutions (5 mg/mL and 10 mg/mL) are designated as PMMA/GO@HPCTP-1 and PMMA/GO@HPCTP-2, respectively. The numbering method of PMMA/C60@HPCTP and PMMA/CNTs@HPCTP samples is the same.

3. Results and Discussion

3.1. Structural analysis of materials

Figure 1 reveals the FT-IR spectra of different materials. In the spectra of GO@HPCTP, C60@HPCTP, and CNTs@HPCTP, the stretching vibration peak near 1630 cm-1 corresponds to the C=C bonds in the carbon nanomaterials, while the O-H stretching vibration peak observed around 1050 cm-1 is attributed to hydroxyl groups formed during the oxidation of them. The C=O stretching vibration peak centered at 1730 cm-1 originates from ester linkages formed through the esterification reaction between carboxyl groups in oxidized carbon nanomaterials and phenoxy groups of HPCTP, whereas the characteristic absorption peak at 1170 cm-1 reflects the formation of P-O-C bonds resulting from the chemical interaction between phosphazene rings and oxygen-containing functional groups in the CNTs, GO, and C60. In the spectra of PMMA/GO@HPCTP, PMMA/C60@HPCTP, and PMMA/CNTs@HPCTP, there are three groups of characteristic peaks consistent with pure PMMA: the distinctive absorption peak of ester groups at 1730 cm-1 and the C-H stretching vibration band at 2950 cm-1, and the hydroxyl stretching vibration peak in the vicinity of 3500 cm-1, indicating that the main components of the three are PMMA. At the same time, the characteristic peaks of the hydroxyl group (1050 cm-1) and C=C (1630 cm-1) in GO, C60O, and O-CNTs also exist in the spectral pattern of the three composites. However, the absorption peak of C=O (1730 cm-1) in modified HPCTP is not shown separately because it is covered up by the characteristic peak of ester groups in PMMA. In addition, the peak of P-O-C (1170 cm-1) can also be found in the spectra of PMMA/GO@HPCTP, PMMA/C60@HPCTP, and PMMA/CNTs@HPCTP, demonstrating the existence of modified HPCTP in the PMMA matrix.

FTIR spectrum of different materials.
Figure 1. FTIR spectrum of different materials.

3.2. Thermal stability analysis

The thermal weight loss curves of different materials have been shown in Figure 2, and the associated data have been provided in Table 1, which includes the initial decomposition temperature (indicated by 5% weight loss, T₅%), the maximum weight loss rate and its corresponding temperature are expressed by Tonset, Umax, and Tmax, respectively.

(a) TG and (b) DTG curves of different composites.
Figure 2. (a) TG and (b) DTG curves of different composites.
Table 1. Data of TGA.
Sample Tonset (°C)

Tmax

(°C)

Umax

(%/°C)

Amount of char residues (500°C) (wt%)
PMMA 185 254 0.68 0.6
PMMA/CNTs@HPCTP-1 194 386 0.92 1.7
PMMA/CNTs@HPCTP-2 191 402 0.96 2.8
PMMA/GO@HPCTP-1 192 388 0.95 2.0
PMMA/GO@HPCTP-2 192 401 0.99 3.4
PMMA/C60@HPCTP-1 190 389 0.99 2.4
PMMA/C60@HPCTP-2 191 403 0.94 3.8

With the admixture of modified HPCTP, the primary disintegration temperature (Tonset) of the composites increases. But the increase is generally small, and there is no significant difference in the Tonset value of different composites. After adding HPCTP, the viscosity of the polymerization system increases during the preparation process, resulting in uneven stirring, and the prepared composites contain more impurities such as water and solvent. Despite thorough purification, trace residual solvents (e.g., THF) or unreacted monomers persist in the composites. These impurities act as plasticizers, lowering Tonset values when the samples are heated.

In marked contrast, the maximum weight loss temperature (Tmax) of the composites exhibited greater variability. The differential thermogravimetry (DTG) curves revealed substantial rightward shifts in exothermic peak positions compared to pristine PMMA. Both carbon materials and HPCTP can promote the emergence of carbon layer on the exterior of PMMA matrix, which hinders the heat and mass transfer. At the same time, the carbon nanomaterials can form a crosslinking network inside the material, inhibiting the heat convection in the matrix and delaying the thermal decomposition of PMMA, which makes the value of Tmax increases with the augmentation of the fraction of flame retardant. Arising from the combined effect of the carbon layer on the surface and the crosslinking network in the matrix, the breaking of the unsaturated double bond at the end of PMMA molecules (as shown in Eq. (1)) is delayed.

When the temperature rises to Tmax, the C-C bonds on the main chain (as shown in Eq. (2)) and the unsaturated double bonds at the end are broken almost simultaneously, resulting in rapid decomposition of the materials.

Therefore, the utmost weight loss rate of the composites appears at the third weight loss peak, and the peak values are much higher than those of the second one.

In addition, the char residue increases with the addition of modified HPCTP, further demonstrating the improvement in the material’s thermal stability. This trend also indicates that modified HPCTP can catalyze increased char formation of PMMA, acting as a more effective physical barrier during combustion, while correspondingly reducing the generation of volatile flammable substances.

3.3. Flame retardant performance analysis

The LOI of PMMA/GO@HPCTP, PMMA/C60@HPCTP, and PMMA/CNTs@HPCTP have been shown in Figure 3. All LOI values were derived from ‌triplicate measurements‌ for each sample. And the standard deviations across replicates were displayed as error bars on the corresponding bar charts.

LOI of different composites.
Figure 3. LOI of different composites.

Relative to pure PMMA, the LOI of the composites is greatly improved after adding modified HPCTP. Among them, the PMMA/C60@HPCTP-2 sample has the highest LOI value (25.8%), which is 47.4% greater than that of pure PMMA, indicating that the incorporation of modified HPCTP can significantly elevate the minimal oxygen concentration required for PMMA combustion. This is because HPCTP can produce non-flammable gases, including N2 and water vapor, during the combustion process, which reduces the oxygen concentration in the gas phase and makes the LOI value of the sample increase markedly.

Figure 4 displays the outcomes of the cone calorimeter test for the composites, and the associated data have been detailed in Table 2. All cone calorimetry data were derived from single measurements.

(a) HRR and (b) THR curves of different materials.
Figure 4. (a) HRR and (b) THR curves of different materials.
Table 2. Data of cone calorimeter test.
Sample pHRR (kW/m2) THR (MJ/m2)
PMMA 951.2 111.5
PMMA/CNTs@HPCTP-1 663.0 67.0
PMMA/CNTs@HPCTP-2 542.3 44.8
PMMA/GO@HPCTP-1 597.1 60.2
PMMA/GO@HPCTP-2 491.1 41.4
PMMA/C60@HPCTP-1 555.2 54.0
PMMA/C60@HPCTP-2 437.6 35.8

As can be observed from Figure 4 and Table 2, the addition of modified HPCTP resulted in decreased peak heat release rate (pHRR) and total heat release (THR) for PMMA, and the ignition time was significantly delayed. Among the samples, PMMA/C60@HPCTP-2 has the optimal flame-retardant performance. Its pHRR is only 437.6 kW/m2, which is 54.0% lower than that of pure PMMA (pHRR=951.2 kW/m2), and its THR is as low as 35.8 MJ/m2, which is 67.9% lower than that of pure PMMA (THR=111.5 MJ/m2). It shows that the mixing of modified HPCTP can reduce the amount of PMMA involved in combustion, so that the instantaneous heat release rate and the THR during combustion are markedly reduced. Furthermore, it can be found that the pHRR and THR values of the three types of composites decrease with the increase of the fraction of modified HPCTP. Taking PMMA/C60@HPCTP for example, the pHRR of PMMA/C60@HPCTP-1 is 555.2 kW/m2. When the content of C60@HPCTP increases, the HRR curve of PMMA/C60@HPCTP-2 not only shows a decrease in peak value but also a narrowing of peak shape, indicating that both the combustion intensity and time of severe combustion decrease. In addition, due to the presence of phosphorus in modified HPCTP, a dense isolated carbon layer can be generated at the onset of combustion, which inhibits the pyrolysis of PMMA as well as the release of combustible gas, thereby significantly delaying the ignition time of the composites.

Comparing the effects of modified HPCTP on the combustion behavior of PMMA, it can be found that PMMA/C60@HPCTP has the lowest pHRR and THR values at the same addition amount. This is because the flame-retardant effect of GO and CNTs is mainly in the condensed phase, while C60, in addition to a flame-retardant performance in the condensed phase, has outstanding free radical scavenging ability at the same time, which enables it to have excellent flame-retardant performance in the gas phase.

Compared with our previous studies [25,26] where carbon nanomaterials served as flame retardants of PMMA alone, the PMMA/CNTs@HPCTP composite at maximum loading demonstrates a 20% increase in LOI (24.6% vs. 20.5% for PMMA/CNTs) alongside a 27.8% reduction in pHRR (542.3 kW/m2 vs. 750.9 kW/m2 for PMMA/CNTs), while PMMA/C60@HPCTP exhibits a 12.8% LOI enhancement and 21.5% pHRR decrease relative to PMMA/C60. Notably, standalone HPCTP typically requires >10% loading to achieve comparable flame retardancy, yet its integration with carbon nanomaterials significantly amplifies efficiency, a disparity that collectively demonstrates robust synergistic interactions between HPCTP and nanocarbons, thereby validating the superior flame-retardant performance of modified HPCTP.

Literature analysis reveals that phosphorus-nitrogen synergistic flame retardants typically require additive loadings exceeding 10 wt% to achieve satisfactory flame retardancy. For instance, Yi et al. [27] reported a 14 wt% additive dosage of Dimethyl methylphosphonate/Methacrylamide (DMMP/MAM) yielding an LOI value of 23.1% with 27.0% and 19.9% reductions in pHRR and THR, respectively. While carbon nanomaterials demonstrate notable flame-retardant improvements at lower additive levels (e.g., 3 wt% graphene achieving a 16.9% pHRR reduction according to Ref. [28]), their performance plateaus higher concentrations due to inherent agglomeration issues. In contrast, this study introduces a novel carbon nanomaterial-modified HPCTP system that synergistically addresses these limitations. The HPCTP matrix not only enhances nanomaterial dispersion to prevent agglomeration but also activates a tri-elemental (nitrogen-phosphorus-carbon) synergy, significantly surpassing conventional single-component or dual-element strategies. This integrated approach achieves superior flame retardancy in PMMA at reduced additive loadings, as evidenced by the data above, positioning it as a benchmark for next-generation flame-retardant polymer design.

3.4. Analysis of the flame-retardant mechanism

3.4.1. Morphology analysis of char residues

SEM images of residues produced by PMMA composites have been displayed in Figure 5. Compared with the char residue of pure PMMA shown in Figure 5(a), the char residues in Figures 5(b-d) are more compact, and a dense cross-linked network is formed by carbon nanomaterials on the surface, which results in a more significant physical isolation effect on heat and gas during combustion. In Figure 5(b), more blocks can be found on the exterior of the char residue, which are agglomerates formed with CNTs, indicating an uneven dispersion of CNTs even with the presence of HPCTP. These agglomerations negatively impact flame retardancy by disrupting the continuity of the graphitized char layer, thereby reducing its insulating capacity, and limiting the accessible surface area for synergistic radical scavenging with HPCTP, as reflected in the slightly elevated pHRR values compared to PMMA/GO@HPCTP and PMMA/C60@HPCTP. Compared with CNTs, the GO distribution on the surface of carbon residue (Figure 5c) is more uniform, the aggregates are reduced, and only a small number of voids exist. Compared with the previous two, no obvious voids are observed in Figure 5(d). C60 forms a uniform and dense network structure in the char residue, which can effectively block the transfer of heat, oxygen, and combustible gases, and creates a flame-retardant effect.

SEM images of residues produced by (a) PMMA, (b) PMMA/CNTs@HPCTP, (c) PMMA/GO@HPCTP, and (d) PMMA/C60@HPCTP.
Figure 5. SEM images of residues produced by (a) PMMA, (b) PMMA/CNTs@HPCTP, (c) PMMA/GO@HPCTP, and (d) PMMA/C60@HPCTP.

The SEM images were converted into binary format through threshold segmentation, followed by quantitative porosity analysis using ImageJ software (calculated as pore area/total area × 100%). The measured porosity values of 62.8%, 25.7%, 24.0%, and 27.7% correspond to Figure 5(a-d) respectively. These findings conclusively demonstrate that the PMMA composites developed a significantly denser char layer with a predominant closed-cell structure during combustion. This optimized microstructure, characterized by reduced open porosity and enhanced cellular integrity, maintains sustained thermal barrier functionality throughout combustion, effectively retarding heat/mass transfer while resisting structural collapse under thermal stress.

The comparative analysis of char residue morphology and flame-retardant parameters establishes a significant correlation: denser carbonaceous structures with reduced porosity (<30%) correspond to enhanced composite performance metrics, including higher LOI, lower pHRR, and THR values compared to pure PMMA.

3.4.2. XPS investigation of char residues

The XPS spectra of charred materials by PMMA composites have been shown in Figure 6, in which data of samples with the largest fraction of modified HPCTP (PMMA/CNTs@HPCTP-2, PMMA/GO@HPCTP-2, PMMA/C60@HPCTP-2) are selected for comparison.

XPS spectra of char residues produced by PMMA/modified HPCTP composites.
Figure 6. XPS spectra of char residues produced by PMMA/modified HPCTP composites.

From Figure 6, it is evident that the char residue of pure PMMA does not contain P and N. After adding modified HPCTP, a small amount of P and N appear in the char residues, and the content of P is higher. The relative content of each element has been displayed in Table 3.

Table 3. The relative content of each element in the carbon residues.
Sample Content (At%)
C O P N
PMMA 69.51 30.49 / /
PMMA/CNTs@HPCTP-2 78.36 18.11 2.68 0.85
PMMA/GO@HPCTP-2 80.29 16.16 2.72 0.83
PMMA/C60@HPCTP-2 82.44 13.83 2.85 0.88

One can observe from Table 3 that the content of C in the carbon residues increases after adding modified HPCTP, indicating that it can catalyze more PMMA to dehydrate into carbon. At the same time, P in HPCTP can combine with O in the composites and generate PO· and PO2˙, which reduces the content of O in the condensed phase. These free radicals can capture ·H and ·OH radicals produced by the decomposition of PMMA in the gas phase, thereby interrupting the chain radical reaction of PMMA. In addition, the atomic ratio of P and N (P/N) in HPCTP is 1:1, while the P/N ratios in PMMA/CNTs@HPCTP, PMMA/GO@HPCTP, and PMMA/C60@HPCTP are measured as 3.15, 3.28, and 3.24, respectively. A higher P/N ratio correlates with phosphorus enrichment in the condensed phase, promoting char-layer crosslinking and compact char formation to establish a physical barrier that suppresses heat transfer and flammable gas diffusion. Concurrently, the reduced nitrogen content in the char residue implies its conversion into inert gaseous species such as N2 and NH3, which enhances gas-phase flame retardancy through dilution and inerting effects.

As a phosphazene flame retardant, P and N in HPCTP have an important influence on the improvement of flame retardancy of PMMA. To more thoroughly examine the bonding state of P and N in the char residues, peaks of the two elements were fitted, as demonstrated in Figure 7.

XPS peak fitting results for the char residues: (a-c) P 2p spectra of PMMA/CNTs@HPCTP, PMMA/GO@HPCTP and PMMA/C60@HPCTP; (d-f) N 1s spectra of PMMA/CNTs@HPCTP, PMMA/GO@HPCTP and PMMA/C60@HPCTP.
Figure 7. XPS peak fitting results for the char residues: (a-c) P 2p spectra of PMMA/CNTs@HPCTP, PMMA/GO@HPCTP and PMMA/C60@HPCTP; (d-f) N 1s spectra of PMMA/CNTs@HPCTP, PMMA/GO@HPCTP and PMMA/C60@HPCTP.

Figure 7(a) reveals that, Figures 7(b), and 7(c) reveal that there are two peaks (132.8 eV and 133.7 eV) in the P 2p peak fitting spectra of char residues produced by PMMA composites. The peak at 132.8 eV is attributed to the P-O-C groups in phosphate, while the peak at 133.7 eV is derived from the P=O bonds in phosphoric and metaphosphoric acid or the P=N bond in HPCTP. The results show that there are phosphoric acid, metaphosphoric acid, and phosphate in the char residues, which are produced by the decomposition of HPCTP. These decomposition products cover the surface of the matrix and have a strong blocking effect on the conveyance of heat and gas. In addition, phosphoric acid and metaphosphoric acid can also promote the dehydration and carbonization of PMMA, which avoids its flame combustion and generates a carbonized layer on the exterior. The carbonization layer and the phosphoric acid coating work together, which makes the resistance to heat and gas transfer increase significantly.

In the N 1s peak fitting spectra shown in Figures 7(d-f), peaks at 398.6 eV and 400.5 eV correspond to -NH- and -N= in HPCTP, respectively. There is only a small amount of N in the form of -N= in the carbon residue, indicating that the phosphazene ring in HPCTP is broken, and most of the N in the phosphazene ring is converted into N2 or other gases and release to the gas phase during the combustion process.

3.4.3. Raman spectrum analysis of carbon residue

Figure 8 indicates the Raman spectra of PMMA composites. Figure 8 illustrates that the Raman spectra of all materials feature two characteristic peaks: 1352 cm⁻1 (D band) and 1592 cm⁻1 (G band). These peaks correspond to the vibrational modes of disordered carbon and graphite carbon, respectively. The graphitization degree of carbon residue is usually represented by the area ratio of the D peak to the G peak, as shown in Eq. (3).

(3) R = A D / A G

(a-d) Raman spectra of the carbon residues.
Figure 8. (a-d) Raman spectra of the carbon residues.

The lower the R value, the higher the degree of graphitization in the carbon layer, and consequently, the enhanced thermal stability.

As shown in Figure 8(a), the R value of pure PMMA is 1.26. After adding modified HPCTP, the R values in Figures 8(b-d) all decrease, indicating a ‌moderate increase in graphitization of the residue. The observed graphitization trend is closely tied to the flame-retardant mechanism: thermally stable graphitic domains reinforce the continuity and mechanical integrity of the carbonaceous layer, forming a compact barrier that suppresses oxygen ingress and heat feedback during combustion. Concurrently, the retained amorphous regions and defects (evidenced by D-band intensity) contribute to radical scavenging and gas-phase inhibition, ensuring a synergistic interplay between condensed-phase and gas-phase flame-retardant mechanisms. Among the three composites, the R value of PMMA/C60@HPCTP is the lowest, which may be related to the fewer defects in the cage structure of C60. Compared with C60, CNTs and GO are more likely to have defects at the edges of their molecules, which results in a diminished level of graphitization and an elevated R value for the corresponding composites.

3.4.4. Synergistic flame-retardant mechanism of carbon nanomaterials and HPCTP

Drawing from the carbon residue analysis, the flame-retardant mechanism of the nitrogen/phosphorus/carbon ternary system, established by carbon nanomaterials and HPCTP, is elucidated, as depicted in Figure 9.

Flame retardant mechanism diagram of N/P modified carbon.
Figure 9. Flame retardant mechanism diagram of N/P modified carbon.

The nitrogen and phosphorus components in HPCTP provide flame-retardant functionality in both the gas and condensed phases. Within the gaseous phase, PO· radicals undergo bimolecular interactions with transient hydrogen radicals (·H) derived from PMMA thermal decomposition and hydroxyl radicals (·OH) formed via ·H/O2 reactions. This synergistic radical quenching mechanism disrupts the free radical chain reaction of PMMA, thereby effectively suppressing self-sustaining flame propagation. At the same time, the decomposition products of HPCTP, such as water vapor, N2, and other non-combustible gases, reduce the degree of flammable substances in the gas phase, so that the combustion is weakened or even extinguished. In the condensed phase, the phosphoric acid and phosphate produced by the thermal decomposition of phosphorus form a covering layer on the surface of the matrix, while promoting the dehydration of PMMA and forming a carbon layer. The non-combustible gases, such as water vapor, generated by its decomposition, can form bubbles in the carbon layer, which results in the carbon layer expanding and thickening. This carbon layer can prevent heat from entering the matrix and prevent the combustible gas from escaping to the gas phase, thereby interrupting the combustion.

When HPCTP is modified by carbon nanomaterials, the modified flame retardants have the blocking effect of phosphorus flame retardants in the condensed phase, the free radical capture effect in the gas phase, and the dilution and inerting effect of nitrogen flame retardants in the gas phase. In addition, C60 can synergistically capture combustible free radicals with PO·, while the cross-linked network structure formed by CNTs, GO and C60 inside and on the surface of PMMA matrix can synergistically form an insulating layer with the phosphorus flame-retardant agent in the solid phase, which more completely blocking the transfer of heat and oxygen. According to the experimental results, it can be concluded that the condensed-phase barrier effect plays the dominant role in flame retardancy, as evidenced by the formation of a continuous graphitized char layer and a significant reduction in pHRR, while gas-phase radical scavenging exhibits a secondary contribution due to minimal changes in TGA.

4. Conclusions

After adding modified HPCTP, the temperature at which the maximum weight loss rate occurs for each PMMA composite is notably elevated, and the thermal stability of the PMMA composites is improved. Simultaneously, the limit oxygen index (LOI) of the composite is up to 25.8% (PMMA/C60@HPCTP-2), representing a 47.4% increase compared to pure PMMA. Meanwhile, the pHRR and THR are reduced by 54.0% and 67.9%, respectively. Analytical characterization of the char residues through SEM images, XPS, and Raman spectroscopy revealed that the composites formed a more compact and continuous char structure with an elevated degree of graphitization compared to pure PMMA. The presence of phosphoric acid, metaphosphoric acid, and phosphate derivatives within the char layer created an effective barrier interface on the PMMA surface, exerting a robust physical shielding effect against heat transfer and gaseous diffusion between the matrix and its surroundings. These findings conclusively demonstrate the synergistic flame-retardant interaction among nitrogen, phosphorus, and carbon, ultimately leading to significantly enhanced fire resistance in the PMMA composites.

While modified HPCTP demonstrates advantages such as low additive loading and high flame-retardant efficiency, the scaled production of its nanocarbon components relies on high-temperature chemical vapor deposition (CVD) or intricate chemical modification processes, entailing substantially higher production costs compared to conventional flame retardants. Additionally, the stringent requirement for precise dispersion control during processing further elevates the complexity of the manufacturing workflow. Moreover, the incorporation of nanocarbon materials may substantially compromise critical material properties, including optical transparency and mechanical flexibility. In practical application, suitable types of flame retardants can be selected according to various factors such as economy, ease of production and processing, thermal stability, flame retardancy, etc. For instance, while CNTs@HPCTP exhibits suboptimal flame-retardant efficacy, its mature fabrication processes and cost-effectiveness render it suitable for applications where stringent flame resistance is not critical. Conversely, C60@HPCTP, despite its higher cost, demonstrates superior dispersibility and optimal flame-retardant performance, making it the preferred choice for high-demand scenarios requiring substantial flame-retardant loadings.

Although pre-treatment strategies such as oxidation and ultrasonic dispersion were employed for the carbon nanomaterials, coupled with the utilization of HPCTP to further enhance their dispersion, varying degrees of agglomeration were still observed at higher loading levels. For future research, the chemical modification of nanocarbon materials using flame-retardant surfactants merits further investigation. This approach could enhance dispersion stability at elevated filler loadings, thereby allowing higher flame-retardant additive concentrations to improve the fire resistance of PMMA composites. Furthermore, systematic investigations into the quantitative relationships between flame-retardant dosage and the mechanical properties, thermal stability, and flame-retardant efficiency of PMMA would provide critical insights for optimizing multifunctional performance in practical applications.

Acknowledgment

This work was supported by the Scientific Research Foundation of Shandong University of Aeronautics (No. 2023Y40) and the Graduate Innovation Foundation of Shandong University of Aeronautics (No.SHSYCX09)

CRediT authorship contribution statement

Lanjuan Xu: Writing-original draft, Validation, Investigation, Formal analysis, Funding acquisition. Xinlei Jia: Formal analysis, Conceptualization. Yingying Hu: Methodology, Writing-review & editing. Qing Cao: Validation, Writing-review & editing. Yonghui Wang: Investigation,Funding acquisition.

Declaration of competing interest

The authors declare that they have no known competing financialinterests or personal relationships that could have appeared to influencethe work reported in this paper.

Declaration of Generative AI and AI-assisted technologies in the writing process

The authors confirm that there was no use of artificial intelligence (AI)-assisted technology for assisting in the writing or editing of the manuscript and no images were manipulated using AI.

References

  1. , , , . Carbon-family materials for flame retardant polymeric materials. Progress in Polymer Science. 2017;69:22-46. https://doi.org/10.1016/j.progpolymsci.2017.02.001
    [Google Scholar]
  2. , , , , , . Recent advances in carbon-based nanomaterials for flame retardant polymers and composites. Composites Part B: Engineering. 2021;212:108675. https://doi.org/10.1016/j.compositesb.2021.108675
    [Google Scholar]
  3. , , , , , . Enhanced thermal conductivity and satisfactory flame retardancy of epoxy/alumina composites by combination with graphene nanoplatelets and magnesium hydroxide. Composites Part B: Engineering. 2016;98:134-140. https://doi.org/10.1016/j.compositesb.2016.04.062
    [Google Scholar]
  4. , , , , . Synergistic flame retardancy effect of graphene nanosheets and traditional retardants on epoxy resin. Composites Part A: Applied Science and Manufacturing. 2016;89:26-32. https://doi.org/10.1016/j.compositesa.2016.03.012
    [Google Scholar]
  5. , , , , . Magnesium hydroxide/graphene oxide chip in flakes structure and its fire-retardant reinforcement of polypropylene. Journal of Polymer Research. 2021;28:393-402. https://doi.org/10.1007/s10965-021-02764-y
    [Google Scholar]
  6. , , , , , , . Comparative study on the synergistic effect of POSS and graphene with melamine phosphate on the flame retardance of poly(butylene succinate) Thermochimica Acta. 2012;543:156-164. https://doi.org/10.1016/j.tca.2012.05.017
    [Google Scholar]
  7. , , , , , . Synergistic effect of graphene oxide and boron-nitrogen structure on flame retardancy of natural rubber/IFR composites. Arabian Journal of Chemistry. 2020;13:6274-6284. https://doi.org/10.1016/j.arabjc.2020.05.016
    [Google Scholar]
  8. , , , , , , . Graphene doped Sn flame retardant prepared by ball milling and synergistic with hexaphenoxy cyclotriphosphazene for epoxy resin. Journal of Materials Research and Technology. 2022;17:774-788. https://doi.org/10.1016/j.jmrt.2022.01.017
    [Google Scholar]
  9. , , , , , , . Synergistic effects of graphene and ammonium polyphosphate modified with vinyltrimethoxysilane on the properties of high-impact polystyrene composites. Polymers. 2021;13:881. https://doi.org/10.3390/polym13060881
    [Google Scholar]
  10. , , , , , . Synergistic flame-retardant effect of epoxy resin combined with phenethyl-bridged DOPO derivative and graphene nanosheets. Chinese Journal of Polymer Science. 2019;37:79-88. https://doi.org/10.1007/s10118-019-2175-6
    [Google Scholar]
  11. , , , , , . Synergistic effects of hybrid nanofillers on graphene oxide reinforced epoxy coating on corrosion resistance and fire retardancy. Journal of Applied Polymer Science. 2022;139:51640-51651. https://doi.org/10.1002/app.51640
    [Google Scholar]
  12. , , , , , . The influences of graphene and carbon nanotubes on properties of waterborne intumescent fire resistive coating. Powder Technology. 2021;385:572-579. https://doi.org/10.1016/j.powtec.2021.03.018
    [Google Scholar]
  13. , , , . Detailed kinetic analysis of slow and fast pyrolysis of poly(methyl methacrylate)-Flame retardant mixtures. Thermochimica Acta. 2020;687:178545. https://doi.org/10.1016/j.tca.2020.178545
    [Google Scholar]
  14. , , , , , , , , . Flame-Retardant and Transparent Poly(methyl methacrylate) Composites Based on Phosphorus-Nitrogen Flame Retardants. ACS Appl Polym Mater. 2022;5:846-855. https://doi.org/10.1021/acsapm.2c01786
    [Google Scholar]
  15. , , . Synthesis and characterization of a novel epoxy resin based on cyclotriphosphazene and its thermal degradation and flammability performance. Polymer Degradation and Stability. 2014;109:240-248. https://doi.org/10.1016/j.polymdegradstab.2014.07.020
    [Google Scholar]
  16. , , , . Preparation of halogen-free flame-retardant expandable polystyrene foam by suspension polymerization. Journal of Applied Polymer Science. 2019;136:47779-47788. https://doi.org/10.1002/app.47779
    [Google Scholar]
  17. , , , . Phosphazene as an effective flame retardant for rapid curing epoxy resins. Reactive and Functional Polymers. 2021;164:104910. https://doi.org/10.1016/j.reactfunctpolym.2021.104910
    [Google Scholar]
  18. , , , , , , . Preparation of continuous glass fiber/polyamide 6 composites containing hexaphenoxycyclotriphosphazene: Mechanical properties, thermal stability, and flame retardancy. Polymer Composites. 2022;43:1022-1037. https://doi.org/10.1002/pc.26431
    [Google Scholar]
  19. , , , , , . Preparation and characterization of ethylene–vinyl acetate copolymer (EVA)–magnesium hydroxide (MH)–hexaphenoxycyclotriphosphazene (HPCTP) composite flame-retardant materials. Polymer Bulletin. 2019;76:2399-2410. https://doi.org/10.1007/s00289-018-2500-1
    [Google Scholar]
  20. , , , , , , . A study on flame retardancy and smoke suppression of diatomite/hexaphenoxycyclotriphosphazene in silicone rubber foam. J Rubber Res. 2023;26:407-413. https://doi.org/10.1007/s42464-023-00224-4
    [Google Scholar]
  21. , , , , , . TGA-FTIR and char residue analysis: Studying the synergistic flame retardancy mechanism of ionic liquid-modified graphene and hexaphenoxy cyclotriphosphazene. J Therm Anal Calorim. 2022;147:13253-13259. https://doi.org/10.1007/s10973-022-11615-x
    [Google Scholar]
  22. , , , , , , , . Fabrication and Characterization of PMMA/MWCNTs Composite Materials. Journal of Wuhan University of Technology-Materials Science Edition. 2023;38:1190-1197. https://doi.org/10.1007/s11595-023-2809-y
    [Google Scholar]
  23. , , , , . Fabrication of a high fire safety, transparent coating for polymethylmethacrylate with superior hardness and adhesion. Progress in Organic Coatings. 2022;172:107079. https://doi.org/10.1016/j.porgcoat.2022.107079
    [Google Scholar]
  24. , , , , , , , , , , , . Rheological, flame retardancy, and thermomechanical properties of polymethyl methacrylate composites: Effects of flame retardant and toughener. Journal of Applied Polymer Science. 2022;139 https://doi.org/10.1002/app.52418
    [Google Scholar]
  25. , , , , , , . Preparation and study on the flame-retardant properties of CNTs/PMMA microspheres. ACS Omega. 2021;7:1347-1356. https://doi.org/10.1021/acsomega.1c05606
    [Google Scholar]
  26. , , , , . Preparation and study of the flame retardant properties of C60/PMMA microspheres. RSC Advances. 2022;12:22623-22630. https://doi.org/10.1039/d2ra03642h
    [Google Scholar]
  27. , , , , , , , , . Flame-retardant and transparent poly(methyl methacrylate) composites based on phosphorus-nitrogen flame retardants. ACS Appl Polym Mater. 2023;5:846-855. https://doi.org/10.1021/acsapm.2c01786
    [Google Scholar]
  28. , , , . Experimental study of the flame retardancy of PMMA-graphene composite materials. Engineering, Technology & Applied Science Research. 2024;14:13324-13328. https://doi.org/10.48084/etasr.6883
    [Google Scholar]
Show Sections