Abstract
Zinc-containing solid wastes (ZCSW) from the steel industry pose significant environmental risks due to hazardous heavy metals like zinc, iron, and lead. This study proposes a synergistic ammonia-acid leaching strategy for co-processing blast furnace dust (BFD) and secondary zinc oxide (SZO) to achieve resource recovery and pollution mitigation. The ammonia leaching selectively extracted 70.62–88.08% of Zn while suppressing Fe and Pb dissolution, facilitated by optimized (NH3·H2O]/[NH4HCO3] ratios (1:1) and pH (9.84). Subsequent acid leaching (3.24 mol·L-1 HCl, 50°C) effectively dissolved residual Zn (95.7%) and Pb by leveraging BFD’s reducibility to oxidize refractory ZnS in SZO. Selective metal recovery was achieved through pH-controlled precipitation: Fe3⁺ was removed as Fe2O3 at pH 5, Pb via Zn displacement, and ZnCO3 via ammonium bicarbonate addition. The integration of BFD enhanced ZnS leaching efficiency, while mixed waste ratios (e.g., 3:1 BFD/SZO) optimized elemental separation, converting residues into Fe-enriched (73.42%) materials. This waste-to-waste approach enables simultaneous Zn, Fe, and Pb recovery with <1% residuals, offering a sustainable solution for ZCSW management by bridging resource scarcity and environmental challenges.
Keywords

1. Introduction
Zinc-containing solid waste (ZCSW) primarily arises from major waste emitters within the steel industry [1-3], predominantly containing hazardous heavy metals such as Zn, Fe, and Pb [4-6]. The ZCSW are classified as dangerous national waste categories and represent a significant environmental and health risk if discharged at will [7]. According to statistics, the global steel industry generates approximately 80 million tons of byproducts such as zinc-containing dust annually [8]. As the largest producer of steel in the world, China’s crude steel output reached 1.019 billion tons in 2023, representing 53.85% of global production. The associated zinc-containing solid waste is estimated at 20 to 30 million tons per annum [9]. However, China’s existing zinc ore reserves are limited, totaling approximately 44 million tons. In 2023, zinc production reached 7.15 million tons, with roughly 70% sourced from primary ore smelting and only about 30% derived from secondary resource recycling [9]. Currently, a significant portion of zinc-containing solid waste is still managed through stacking or landfill disposal methods, contributing to severe land and water pollution issues [10,11].
Blast furnace dust (BFD), a form of ZCSW, is generated during steel smelting, consists of fine particles carried along with blast furnace gas through gravity dust removal and baghouse ash collection [12,13]. The production of each ton of pig iron generates approximately 20–30 kg of BFD [14]. It primarily contains iron oxides and low levels of metal oxides such as Pb and Zn [15]. Secondary zinc oxide (SZO), derived from the pyrometallurgical enrichment of BFD using rotary kilns or shaft furnaces, contains substantial amounts of zinc along with some iron and lead metals, rendering direct utilization unfeasible [16-18].
Promoting the recovery of zinc from solid waste not only helps reduce the pressure on zinc supply but also plays a vital role in achieving clean production and sustainable development in the steel industry [19]. It is essential to develop efficient and eco-friendly recycling processes to enhance the circular utilization of zinc resources and minimize environmental risks.
To summarize, this study investigates the synergies between two common forms of ZCSW, BFD and SZO, using an ammonia-acid leaching method for simultaneous treatment. Selective large-scale enrichment of zinc metal elements can be achieved by regulating BFD and SZO with different mass ratios; especially owing to the oxidation properties of BFD, zinc sulfide in SZO can be effectively leached by acid in mixed samples. The paper focused on elucidating the complex leaching of lead from zinc ash and the directed separation of heavy metals, zinc, iron, and lead through pH regulation, and provided insights into the mechanism of the entire process. Through a synergistic treatment strategy that utilizes “waste to treat waste,” BFD is not only seen as a material that requires disposal but is also repurposed as a functional resource. It provides the necessary Fe3+ oxidizing agent that enhances the dissolution of ZnS in SZO during the acid leaching process. This enables a synergistic recovery process that requires no additional oxidant and is more cost-effective. Simultaneously, a closed-loop system enables the transformation of hazardous solid waste into valuable metal products. This research presents a win-win solution for the combined treatment of BFD and SZO, improving the efficiency of metal resource recovery while reducing the management challenges associated with zinc smelting residues.
2. Materials and Methods
2.1. Materials
In the iron smelting process, the blast furnace gas undergoes primary dedusting via a gravity dust collector to eliminate coarse particles. This is followed by secondary dedusting using bag filtration to isolate finer particles, yielding clean gas. The latter, referred to as BFD, undergoes treatment through the rotary kiln to produce SZO. For this study, BFD and SZO were randomly procured from a steel plant in Yunnan Province. Prior to experimentation, both samples were dried at 105°C for 24 h and then sieved through a 100-mesh screen. Both SZO and BFD contain elements such as Zn, Fe, and Pb. The primary distinction between BFD and SZO lies in their differing elemental compositions, attributable to varying production stages. In this experiment, BFD and SZO were reconstituted into new samples using different mass ratios to optimize leaching effects. Detailed information on the blending method is available in Appendix S1. The elemental composition of the raw materials for B&S-0-1 and B&S-1-0 has been presented in Table S1, while their phase composition has been illustrated in Figure S1.
2.2. Ammonia immersion experiment
Under the conditions of a total ammonia concentration of 6 mol·L-1, a [NH3·H2O]/[NH4HCO3] ratio of 1:1, a temperature of 40°C, a liquid-to-solid ratio of 6:1, and a stirring speed of 400 rpm, pH was 9.84. Samples were each reacted for 3 h. After leaching, solid residues and ammonia leachates were separated via vacuum filtration (using a 0.45 μm filter). Chemical analysis of the ammonia leachate was conducted to determine the concentration of metal ions and to calculate the leaching efficiency of the elements.
2.3. Hydrochloric acid leaching experiment
Under conditions of hydrochloric acid (0.32-4.86 mol·L-1), a liquid-to-solid ratio of 8:1, and temperatures of 25-75°C, the residues from the ammonia leaching stage were leached for 3 h. Following leaching, solid residues and leachates were separated through vacuum filtration (using a 0.45 μm filter). Chemical analysis of the acid leachate was conducted to determine the concentration of metal ions and calculate the leaching efficiency of the elements.
2.4. Resource recovery
To separate the heavy metals zinc, iron, and lead, the recovery of these elements can be achieved by adjusting the pH of the leachate based on the results of chemical equilibrium simulations. The pH of the acid leachate was adjusted to 5 with 25% ammonia solution to ensure complete precipitation of iron after adding content H2O2. Subsequently, the mixture was centrifuged to separate the iron precipitate from the leachate. The iron precipitate was then placed in a crucible and calcined for 1 h to transform it into a stable iron compound Fe2O3. Zinc was added to displace lead, and the leachate was centrifuged to separate it from the lead. The pH of the leachate was then adjusted to 6 using ammonia solution. Ammonium bicarbonate was added to the filtrate, and the mixture was subjected to rotary evaporation at 80°C for 200 min to obtain a white powdered solid.
2.5. Chemical analysis
The total concentration of metal elements was determined by inductively coupled plasma (ICP). During the reaction, the concentration of zinc, iron, and lead was determined using atomic absorption spectroscopy (AAS). The details of the characterization methods and Chemical equilibrium simulation methods have been presented in Appendix S2. The leaching efficiency of BFD and SZO was calculated according to Formula (1). The concentration of iron ions was determined using the orthophenanthroline spectrophotometric method.
(1)
F stands for metal leaching rate (%), C for the heavy metal ion concentration in the solution (mg·L-1), V for the solution’s volume (L), m for the sample’s mass (mg), and w for the heavy metal content percentage (%).
3. Results and Discussion
3.1. Characterization of the original materials
The microstructure of the original materials B&S-1-0 (BFD) and B&S-0-1 (SZO) surfaces was observed by SEM-EDS. Figures 1(a,b) reveal that B&S-1-0 features irregular laminar structures. Regions with a higher iron concentration appear smoother compared to areas where zinc predominates, which are characterized by smaller, adherent flakes or particles. Figure 1(c) clearly shows Zn and Fe as the predominant elements in B&S-1-0, with Pb present in smaller amounts. Figures 1(d,e) show that B&S-0-1 was primarily composed of prismatic bodies and irregularly shaped small particles. Figure 1(f) reveals that Zn is the principal element in B&S-0-1, accompanied by lesser quantities of Fe and Pb. Hence, the primary distinction between B&S-1-0 and B&S-0-1 samples is significantly higher iron content in B&S-1-0.

3.2. Ammonia immersion section
As illustrated in Table S1, systematic evaluation of mixed zinc ash prepared with varying BFD/SZO ratios revealed distinct leaching behaviors. Following ammonia leaching, all samples exhibited significant zinc content reduction, with residual zinc mass fractions ranging from 10.22% to 38.84%. Concurrently, iron and lead concentrations approximately doubled, indicating the transformation of zinc-rich solid waste from high-grade to low-grade material. Particularly noteworthy is the elevated lead content in the resulting low-grade residue, which poses potential ecological and human health risks, thereby necessitating effective lead removal measures. Table S2 provides a detailed comparative analysis of metal extraction efficiencies across different mixing ratios. Zinc was consistently extracted as the predominant element, with leaching rates ranging from 70.62% to 88.08% across all formulations. Critical differences in selectivity were observed: samples B&S-1-1 and B&S-1-2 exhibited exclusive zinc extraction, while B&S-3-1 and B&S-1-3 showed co-extraction of lead at rates of 14.16% and 2.28%, respectively. In contrast, B&S-2-1, B&S-1-0, and B&S-0-1 demonstrated simultaneous extraction of iron, calcium, and manganese alongside zinc. These findings conclusively demonstrate that the selectivity of zinc leaching can be precisely modulated through strategic adjustment of BFD/SZO ratios.
Notably, the 3:1 BFD/SZO ratio (B&S-3-1) was identified as optimal, achieving an excellent balance between high zinc extraction efficiency (88.08%) and minimal impurity co-dissolution, while providing sufficient iron content to facilitate subsequent ZnS oxidation during acid leaching. Despite the inherent selectivity of ammonia leaching, minor impurities, including calcium, manganese, iron, and lead, were detected in the leachate. To enhance solution purity, purification protocols including CO2-assisted precipitation of calcium/manganese and zinc cementation for lead removal were implemented (Table S3). As confirmed by Figures S2 and S3, these treatments effectively removed the targeted impurity ions from the ammonia leaching solution.
3.3. Acid immersion section
Further acid leaching of ammonia leaching residue to recover the remaining metal. The experiment was carried out at an acidity of 3.24 mol·L-1, a temperature of 50°C, a liquid-solid ratio of 8:1, and a reaction time of 2 h. Figure 2(a) illustrates the elemental composition evolution of all samples following sequential ammonia-acid leaching. The Aci-B&S-0-1 sample displayed minimal alteration in zinc content proportion, whereas Aci-B&S-1-0 and Aci-B&S-3-1 samples showed complete zinc extraction. This divergence primarily stems from the differential solubility characteristics of zinc compounds in SZO versus BFD, with the latter demonstrating enhanced extractability.

A crucial correlation was established between zinc leaching efficiency and Fe3+ concentration (Figure 2b). As the BFD content decreased systematically from Amm-B&S-3-1 to Amm-B&S-1-3, both Fe3+ concentration and corresponding zinc leaching rates exhibited parallel declines. This strong positive correlation provides compelling evidence that iron compounds derived from BFD play a pivotal role in facilitating zinc compound extraction from mixed zinc ash samples, likely through oxidative dissolution of refractory ZnS phases. Based on comprehensive screening, the 3:1 BFD/SZO mass ratio demonstrated superior performance in the integrated ammonia-acid leaching system, achieving the maximum zinc recovery. Consequently, the B&S-3-1 formulation was selected for detailed investigation of acid leaching parameters.
Systematic optimization of acid leaching conditions was conducted using the Amm-B&S-3-1 residue. As shown in Figures 2(c,d), both acidity and temperature profoundly influenced the extraction dynamics of zinc, iron, and lead. At 0.32 mol·L-1 HCl, lead remained essentially unleached, while iron extraction was substantially limited. Increasing acidity to 1.62 mol·L-1 enabled zinc leaching equilibrium, accompanied by significantly enhanced iron dissolution and lead extraction capacity. Complete leaching equilibrium for all target metals (zinc, iron, and lead) was achieved at 3.24 mol·L-1. Temperature optimization studies revealed minimal extraction at 25°C, with equilibrium attainment at 50°C (Figure S4). Higher temperatures provided no appreciable kinetic advantage. Therefore, the optimal acid leaching conditions were established as 3.24 mol·L-1 HCl at 50°C, corresponding to pH 1.26, which ensured maximized extraction efficiency for zinc and lead from Amm-B&S-3-1. Figure 2(e) conclusively demonstrates the successful resource recovery achieved through sequential leaching: zinc and lead contents in B&S-3-1 were reduced to <1%, while iron was concentrated to 73.42%, effectively transforming industrial solid waste into valuable crude iron ore.
3.4. Sample characterizations after reaction
Changes in the main components during ammonia leaching and acid leaching were studied by X-ray diffraction (XRD). Figure 3(a) illustrates the XRD pattern of samples before ammonia and acid leaching. The B&S-0-1 sample primarily contains ZnS and ZnO, while the B&S-1-0 sample contains Fe2O3, ZnO, hausmannite, and calcite phases. Samples prepared with different compositions exhibit diffraction peaks corresponding to both B&S-0-1 and B&S-1-0. Figure 3(b) shows the XRD pattern of the sample after ammonia leaching. The Amm-B&S-0-1 sample retains an unchanged ZnS diffraction peak, the disappearance of the ZnO diffraction peak, and the emergence of new diffraction peaks corresponding to PbCO3, PbO, and FeO, indicating the extraction of ZnO and the poor solubility of PbCO3, PbO, and FeO in the ammonia system. The Amm-B&S-1-0 sample exhibits diffraction peaks of Fe2O3 and Fe3O4, suggesting substantial dissolution of ZnO, hausmannite, and calcite in the ammonia system. After ammonia leaching, it is observed that mixed zinc ash samples with different compositions encounter difficulties in leaching out PbCO3, PbO, FeO, ZnS, Fe2O3, and Fe3O4 during the ammonia leaching stage. Figure 3(c) presents the XRD pattern of the sample after acid leaching. The Aci-B&S-0-1 sample displays a new diffraction peak corresponding to PbCl2, likely formed due to the presence of PbCO3 and PbO in the acid system, while the ZnS diffraction peak remains unchanged. In the Aci-B&S-1-0 sample, the disappearance of the Fe3O4 diffraction peak leaves only the Fe2O3 and SiO2. As the BFD dosage increased, the characteristic diffraction peaks of sphalerite (ZnS) in the XRD patterns gradually disappeared. This effect is likely attributable to the higher content of iron oxides under acidic conditions, which leads to increased leaching of iron as Fe3+. In the leachate, Fe3+ acts as an oxidant by being reduced to Fe2+, thereby accepting electrons from ZnS and promoting the oxidative dissolution of sphalerite, which increases the sphalerite leaching efficiency [20,21]. In the mixed ash samples, as the proportion of SZO decreases, the intensity of the PbCl2 peak diminishes, disappearing completely in the Aci-B&S-2-1 and Aci-B&S-3-1 samples. Therefore, the ratio of B&S-3-1 is more favorable to achieve complete separation of zinc and lead. Further XRD pattern (Figure 3d) of the Aci-B&S-3-1 sample shows the changes of main components under different acidities. As the acidity gradually increases from 0.32 mol·L-1 to 3.24 mol·L-1, PbCO3 is gradually converted to PbCl2. Under 3.24 mol·L-1 acidity, only peaks corresponding to Fe2O3 and SiO2 are observed, suggesting that this acidity level is necessary for effective leaching of zinc and lead. At the same time, the acid leaching time was also optimized to ensure complete dissolution of zinc (Figure S5).

X-ray photoelectron spectroscopic (XPS) analysis was performed on the B&S-3-1 sample after different treatment stages. The XPS survey spectrum (Figure S6) reveals that during the ammonia leaching stage, the B&S-3-1 sample exhibited peaks corresponding to Zn, Pb, and Fe. However, during the acid leaching stage, the characteristic peaks of Zn and Pb disappeared, while the intensity of the Fe peak increased. This is mainly attributed to the dissolution of Zn and Pb after acid leaching, while Fe, being less soluble, resulted in a relatively higher Fe content. Figure 3(e) shows that the high-resolution Fe 2p spectrum of the B&S-3-1 sample in both the ammonia leaching and acid leaching stages exhibited double peaks for Fe 2p1/2 and Fe 2p3/2, along with satellite peaks. However, compared to Amm-B&S-3-1, Aci-B&S-3-1 showed varying degrees of peak shifts towards lower binding energies. For instance, the main peak of Fe 2p3/2 shifted from 711.87 eV in Amm-B&S-3-1 to 710.92 eV in Aci-B&S-3-1, and the main peak of Fe 2p1/2 shifted from 725.16 eV to 724.31 eV, indicating a decrease in binding energy of approximately 1 eV [22,23]. This suggests a reduction in the oxidation state of high-valent Fe elements. Referring to the above XRD analysis results, further, the Fe2O3 in the B&S-3-1 sample acted as an oxidant during the acid leaching stage, thus promoting the dissolution of ZnS. Furthermore, in Figure 3(f), the Pb4f spectrum exhibited two splitting peaks at 143.71 eV and 138.90 eV, corresponding to the Pb 4f7/2 and Pb 4f5/2 subpeaks, respectively. The peak at 138.90 eV was assigned to stable lead oxides such as PbCO3 and PbO [24]. Additionally, Figure S7 reveals that the Zn 2p3/2 peak was located between 1021-1022 eV, indicating that the zinc compounds in the Amm-B&S-3-1 sample belong to Zn2+ [25]. Through the observations from Figure 3(f) and Figure S7, the signals of Pb 4f and Zn 2p are no longer detectable in the Aci-B&S-3-1 sample, further confirming the successful leaching of Zn and Pb elements in the B&S-3-1 sample. The S 2p XPS analysis depicted in Figure S8 elucidates the transformation pathway of sulfur species throughout the reaction. Post acid leaching, there is a significant reduction in the intensity of the S 2p3/2 peak at 161.90 eV, associated with S2− in metal sulfides (primarily ZnS) [26], suggesting that ZnS is effectively dissolved during the leaching process. Simultaneously, a prominent peak emerges at 164.53 eV, linked to elemental sulfur (S0) [27], confirming the oxidation of ZnS facilitated by Fe3+ from BFD. Additionally, a new peak at 160.81 eV in the leaching residue may represent a small quantity of sulfite or residual sulfide generated during the reaction. All samples show a faint, stable signal around 170.19 eV, which can be attributed to intrinsic sulfate impurities within the initial material [28]. Collectively, these findings indicate that ZnS is transformed into elemental sulfur via an Fe3+-mediated oxidation pathway during acid leaching, alongside a minor side reaction producing sulfate.
To characterize the B&S-3-1 sample after different treatment stages, SEM-EDS analysis was performed. To characterize the B&S-3-1 sample after different treatment stages, SEM-EDS analysis was performed. As depicted in Figures 4(a,b), the surface of the sample exhibited irregularly rough particles after ammonia leaching, and became even more finely fragmented and rough after the acid leaching stage, indicating the leaching of some elements from the B&S-3-1 sample. Moreover, Figure 4b shows that lead was still visibly attached to the sample particles, suggesting the challenge in separating Pb from the sample during the ammonia leaching process. The sample retains a high toxicity, as residual zinc persists in the B&S-3-1 sample even after ammonia leaching, with a content as high as 7.81% (Figures 4c). This implies that the ammonia leaching residue needs to be further extracted. Additionally, Figure 4 (d, e) shows that the distribution of Zn and Pb elements in the Aci-B&S-3-1 sample was not prominent after the acid leaching stage, indicating reduced toxicity of the sample after acid leaching, making this process a viable pathway for the harmless treatment of zinc-containing solid waste. The EDS results presented in Figure 4f indicate that the residue was primarily composed of ferric oxide, with the atomic number ratio of O to Fe being close to 1.5.

3.5. Feasibility process
Figures 5(a-e) demonstrate the feasibility of targeted resource recovery of heavy metals through pH adjustment. Figure 5(a) presents the flowchart for the selective separation of heavy metals in the acid-leaching solution. Initially, a certain amount of hydrogen peroxide was added to oxidize the ferric ion, and the pH of the acid-leaching solution was adjusted to 5 using ammonia water, resulting in the formation of a reddish-brown precipitate. Subsequently, the reddish-brown precipitates were calcined in air, yielding reddish-brown solids. The XRD characterization of the reddish-brown solids has been shown in Figure 5(b), corresponding to Fe2O3 (PDF#72-0469). Zinc blocks were then added to the acid-leaching solution, leading to the formation of black particles. The XRD characterization of the black particles was presented in Figure 5(c), corresponding to Pb (PDF#87-0663). The pH of the acid-leaching solution was further adjusted to 6 using ammonia water, followed by the addition of ammonium bicarbonate as a zinc precipitation agent. This results in the formation of white solids at a certain temperature. The XRD characterization of the white solids is depicted in Figure 5(d), corresponding to Zn5(OH)6(CO3)2 (PDF#72-1100), from Figure S9, it can be observed that the recovery rates of the heavy metals Fe, Pb, and Zn were all above 95%, the purity of ferric oxide was 98.25%, the purity of lead was 90.89%, and the purity of basic zinc carbonate was 97.13%, indicating the achievement of efficient targeted separation and recovery of Fe, Pb, and Zn.

3.6. Chemical equilibrium simulation
According to the simulation results from the Hydra/Medusa software, the chemical speciation distribution of zinc, iron, and lead compounds in the B&S-3-1 sample during ammonia leaching or acid leaching stages concerning pH was illustrated in Figures 5(f-k). The distribution of lead compounds in B&S-3-1 samples during the ammonia leaching stage has been depicted in Figure 5(f). The data show that lead compounds mainly exist in solid forms like lead carbonate or lead hydroxide within the ammonia leaching system at pH levels ranging from 8 to 10.5. This observation is supported by experimental results indicating lead leaching rates consistently below 1% (Table S2) and almost double the lead mass fraction in the residue (Table S1). Furthermore, Figure 5(g) demonstrates that iron is stabilized as Fe2O3 in the ammoniacal system, with experiments showing minimal iron leaching (<1%) and its primary retention in the residue. In contrast, Figure 5(h) reveals that zinc predominantly forms soluble Zn(NH3)42+complexes, with a minor presence of undissolved ZnS [29]. This distribution corresponds to zinc leaching rates varying from 70.62% to 88.08% and residual zinc contents ranging from 10.22% to 38.84%. Theoretical calculations suggest that lead and iron compounds in the B&S-3-1 sample remain insoluble during the ammonia leaching stage, while most zinc compounds form zinc-ammonia complexes and enter the ammonia leaching system, highlighting the necessity for subsequent acid leaching treatment.
During the acidic leaching phase (pH < 2), there is a noticeable alteration in the morphologies of the elements. Lead’s progression from lead carbonate/lead oxide to soluble PbCl22- through PbCl2 intermediates has been depicted in Figure 5(i), aligning with the complete dissolution observed experimentally (residue content < 1%) and validated in Figure S8. The presence of iron primarily as Fe3+ and Fe(OH)2+ ions is shown in Figure 5(j), explaining two experimental findings: the partially solubilized Fe3+ acts as an oxidant, explaining the positive relationship between zinc leaching rate and Fe3+ concentration as depicted in Figure 2(b), while a substantial portion remains in the residue (up to 73.42% Fe). Figure 5(k) affirms that zinc is entirely dissolved as Zn2+. Figures S10-S12 also prove that the dominant regions of lead, iron, and zinc in the acid leaching system are PbCl42-, Fe3+, Fe2+, and Zn2+, respectively. Zinc compounds exhibit good solubility in the acid leaching system, implying that targeted separation of heavy metals Zn, Fe, and Pb in the acid leaching solution can be achieved by controlling the pH value.
Combining the aforementioned characterization and theoretical analysis, The mixed zinc ash B&S-3-1 sample in the ammonia leaching process, ZnO component enters the ammonia leaching system as zinc ammonium complex ion, then Fe2O3 or Fe3O4 component was partially dissolved in acid leaching process, which provides Fe3+ as an oxidant to assist the extraction of ZnS component in the mixed zinc ash, while PbCO3 or PbO was firstly converted into PbCl2 in acid leaching process and then PbCl2 was converted into tolerant PbCl42–, reaction equations R1-R7 can be deduced for the reactions occurring in the ammonia leaching and acid leaching stages of the B&S-3-1 sample.
Simulation results are crucial in guiding pH-controlled separation during the precipitation recovery phase. As shown in Figure 5(j), the most suitable pH range for iron precipitation is 4.5-5.5, facilitating the efficient conversion of soluble Fe3+ to Fe(OH)3 without disruption from different iron hydroxide complexes. Empirical findings validate that over 95% of iron precipitates under these specified circumstances, as depicted in Figure 5(b), while lead remains in the soluble form PbCl42- (Figure 5i), facilitating subsequent replacement recovery. Furthermore, Figure 5(k) illustrates that zinc, during precipitation treatment, remains in the Zn2+ state at pH levels below 6, transitioning to precipitate as Zn5(OH)6(CO3)2 between pH 6.0 and 6.5. This result confirms the feasibility of separating Fe and Pb at lower pH levels before proceeding with Zn precipitation. Both experimental results and simulation predictions underscore the critical importance of precise pH control in the sequential separation of heavy metals. These findings offer a theoretical foundation for optimizing the polymetallic recovery process in complex systems.
The ammonia leaching stage:
R1
The acid leaching stage:
R2
R3
R4
R5
R6
R7
Figure S13 encapsulates the targeted methodological approach of this research. The pretreatment of SZO and BFD involves ammonia complexation followed by simple purification to obtain an ammonia-complexed zinc solution suitable for various applications, such as zinc block preparation or the synthesis of alkaline zinc carbonate via ammonia crystallization. In a synergistic acid leaching step, a specific ratio of SZO and BFD is applied to transform zinc sulfide into zinc chloride and sulfur, while concurrently dissolving some of the iron oxide in the acid. Carbonate lead and lead oxide were transformed into PbCl2 and subsequently to PbCl42- upon interaction with hydrochloric acid, thus yielding an acid leachate containing Zn, Fe, and Pb. The pH of the acid leachate was adjusted using ammonia solution to precipitate iron ions and to facilitate the exchange of lead with zinc blocks, ultimately yielding a zinc-rich solution. This solution was then treated with ammonium bicarbonate to precipitate zinc. Based on the comprehensive process cycle and economic analysis provided in Appendix S3, the proposed selective separation process for recovering heavy metal resources from industrial solid waste demonstrates multiple environmental and economic advantages. These include reduced reagent consumption, procedural simplicity, high solubility of zinc sulfide under ambient conditions, and efficient separation of zinc, iron, and lead.
Although the F2O3, metallic lead, and basic zinc carbonate recovered through this process meet the entry-level requirements of relevant industrial standards and can be recycled as metallurgical and chemical feedstocks, precise control over specific impurities in the products (such as SiO2 and Al2O3 in Fe2O3, zinc in lead, calcium and manganese in basic zinc carbonate) will be the focus of systematic investigation in subsequent studies. In-depth exploration of these issues will provide a critical scientific basis for establishing more precise and economically valuable resource utilization pathways.
4. Conclusions
In summary, the ammonia leaching stage exhibited promising zinc extraction rates exceeding 70% for both SZO and BFD formulations. Notably, selective enrichment of zinc after the ammonia leaching stage can be achieved by adjusting the ratio of BFD and SZO. In the subsequent acid leaching stage, the Fe3+ in the BFD sample effectively promoted the leaching of ZnS in the SZO sample. This innovative approach not only simplifies the process but also contributes to a reduction in industrial solid waste (with a reduction rate of 52.41%). Among the samples, B&S-3-1 demonstrated the most efficient synergistic leaching, resulting in the extraction of the majority of zinc and lead compounds. The leaching slag is coarse-grained iron ore with high utilization potential. The metals were recovered by stepwise separation, with iron ending up as hematite, zinc as alkaline zinc carbonate, and lead as monomers. The recovery of heavy metals Fe, Pb, and Zn by the heavy metal-controlled separation process reached more than 95%, realizing the resourceful utilization of heavy metals from industrial solid waste. Chemical equilibrium simulations were used to calculate the morphology distribution of the mixed zinc ash cascade leach solution, in which zinc oxide enters the ammonia leach system as Zn(NH3)42+, zinc sulfide as Zn2+, iron trioxide as Fe2+ and Fe3+, and lead compounds as either PbCl3- or PbCl42-.
Acknowledgment
This research was financially supported by a project of the National Natural Science Foundation of China [grant numbers 22476171 and 52300140] and Yunnan Fundamental Research Projects (202401AU070028). This research was financially supported by a project of the National Natural Science Foundation of China [grant numbers 22476171 and 52300140] and Yunnan Fundamental Research Projects (202401AU070028).
CRediT authorship contribution statement
Shaoxiang Yang and Yingying Zhong: Design, Manuscript preparation, Literature search, Experimental studies, Data analysis. Jiayu Feng: Design, Manuscript editing and review, Data acquisition. Hanwei Yang: Statistical analysis. Fang Wang: Manuscript editing and review. Futing Xia: Statistical analysis. Shuo Cui: Literature search, Data analysis. Feixiang Lu: Manuscript editing and review. Lijuan Jia: Concepts, Design, and Manuscript editing and review, Validation, Data curation.
Declaration of competing interest
The authors declare that they have no known competing financial interests or personal relationships that could have appeared to influence the work reported in this paper.
Data availability
Data will be made available on request.
Declaration of generative AI and AI-assisted technologies in the writing process
The authors confirm that there was no use of artificial intelligence (AI)-assisted technology for assisting in the writing or editing of the manuscript and no images were manipulated using AI.
Supplementary data
Supplementary material to this article can be found online at https://dx.doi.org/10.25259/AJC_964_2025.
References
- Theoretical study on coal gasification behavior in CO2 atmosphere driven by slag waste heat. Energy. 2024;305:132269. https://doi.org/10.1016/j.energy.2024.132269
- [Google Scholar]
- Enhancement of mixing efficiency in mechanical stirring reactors via chaotic stirring techniques: Application to the treatment of zinc-containing solid waste. Chemical Engineering Science. 2022;249:117367. https://doi.org/10.1016/j.ces.2021.117367
- [Google Scholar]
- Enhancement of in-plant recycling of integrated steel mill offgas solid wastes by reallocating crucial zinc-bearing materials. Journal of Cleaner Production. 2020;251:119783. https://doi.org/10.1016/j.jclepro.2019.119783
- [Google Scholar]
- Leaching of valuable metals from electric arc furnace dust—Tetrabromobisphenol A pyrolysis residues. Journal of Analytical and Applied Pyrolysis. 2017;125:50-60. https://doi.org/10.1016/j.jaap.2017.04.019
- [Google Scholar]
- Selective removal of zinc and lead from electric arc furnace dust by chlorination–evaporation reactions. Journal of Hazardous Materials. 2024;465:133421. https://doi.org/10.1016/j.jhazmat.2023.133421
- [Google Scholar]
- Separation and recovery of zinc, lead and iron from electric arc furnace dust by low temperature smelting. Separation and Purification Technology. 2023;312:123355. https://doi.org/10.1016/j.seppur.2023.123355
- [Google Scholar]
- Current status of hazardous waste disposal technology. IOP Conference Series: Earth and Environmental Science. 2021;760:012034. https://doi.org/10.1088/1755-1315/760/1/012034
- [Google Scholar]
- Synergetic utilization of zinc-bearing dust by carbothermic reduction-roasting process: Phase transformation and morphological evolution. Journal of Sustainable Metallurgy. 2022;8:1090-1103. https://doi.org/10.1007/s40831-022-00554-4
- [Google Scholar]
- Zn recovery strategies from steelmaking dust: A comprehensive review. Separation and Purification Technology. 2025;378:134694. https://doi.org/10.1016/j.seppur.2025.134694
- [Google Scholar]
- Disposal of zinc extraction residues via iron ore sintering process: An innovative resource utilization. Journal of Iron and Steel Research International. 2024;31:1636-1645. https://doi.org/10.1007/s42243-023-01113-1
- [Google Scholar]
- A multilevel sustainability analysis of zinc recovery from wastes. Resources, Conservation and Recycling. 2016;113:88-105. https://doi.org/10.1016/j.resconrec.2016.05.013
- [Google Scholar]
- A review on recycling and reutilization of blast furnace dust as a secondary resource. Journal of Sustainable Metallurgy. 2021;7:340-357. https://doi.org/10.1007/s40831-021-00377-9
- [Google Scholar]
- Review in application of blast furnace dust in wastewater treatment: Material preparation, integrated process, and mechanism. Environmental Science and Pollution Research International. 2024;31:22339-22361. https://doi.org/10.1007/s11356-024-32631-4
- [Google Scholar]
- Recovery of iron and zinc from blast furnace dust using iron-bath reduction. High Temperature Materials and Processes. 2019;38:767-772. https://doi.org/10.1515/htmp-2019-0023
- [Google Scholar]
- A novel approach for the resource utilization of zinc-bearing dust and sludge via the blast furnace main trough. Waste Management (New York, N.Y.). 2023;172:127-139. https://doi.org/10.1016/j.wasman.2023.10.014
- [Google Scholar]
- Pyrometallurgical recovery of zinc and valuable metals from hazardous blast furnace dust via self-reduction roasting: Phase transformations and morphological evolution. Materials Today Sustainability. 2023;24:100590. https://doi.org/10.1016/j.mtsust.2023.100590
- [Google Scholar]
- Pyrometallurgical recovery of zinc and valuable metals from electric arc furnace dust – A review. Journal of Cleaner Production. 2021;298:126788. https://doi.org/10.1016/j.jclepro.2021.126788
- [Google Scholar]
- A review on recycling and reutilization of blast furnace dust as a secondary resource. Journal of Sustainable Metallurgy. 2021;7:340-357. https://doi.org/10.1007/s40831-021-00377-9
- [Google Scholar]
- Research on the impact of circular economy on total factor carbon productivity in China. Environmental Science and Pollution Research International. 2022;29:78780-78794. https://doi.org/10.1007/s11356-022-21314-7
- [Google Scholar]
- A study on the zinc sulfide dissolution kinetics with biological and chemical ferric reagents. Hydrometallurgy. 2017;171:362-373. https://doi.org/10.1016/j.hydromet.2017.06.012
- [Google Scholar]
- Mechanistic modelling of kinetics and mass transfer for a solid–liquid system: Leaching of zinc with ferric iron. Chemical Engineering Science. 2010;65:4460-4471. https://doi.org/10.1016/j.ces.2010.04.004
- [Google Scholar]
- Growth of ultra-thin FeO(100) films on Ag(100): A combined XPS, LEED and CEMS study. Journal of Magnetism and Magnetic Materials. 2014;349:235-239. https://doi.org/10.1016/j.jmmm.2013.08.059
- [Google Scholar]
- Analysis of XPS spectra of Fe2+ and Fe3+ ions in oxide materials. Applied Surface Science. 2008;254:2441-2449. https://doi.org/10.1016/j.apsusc.2007.09.063
- [Google Scholar]
- A porous biochar supported nanoscale zero-valent iron material highly efficient for the simultaneous remediation of cadmium and lead contaminated soil. Journal of Environmental Sciences (China). 2022;113:231-241. https://doi.org/10.1016/j.jes.2021.06.014
- [Google Scholar]
- ZnO surface passivation with glucose enables simultaneously improving efficiency and stability of inverted polymer: Non-fullerene solar cells. Chinese Journal of Polymer Science. 2022;40:1594-1603. https://doi.org/10.1007/s10118-022-2819-9
- [Google Scholar]
- Formation of zinc sulfide species on smithsonite surfaces and its response to flotation performance. Journal of Alloys and Compounds. 2017;709:602-608. https://doi.org/10.1016/j.jallcom.2017.03.195
- [Google Scholar]
- Role of activated carbon in hydroxyl radical production and secondary mineral formation during iron sulfide (FeS) oxidation. Environmental Science & Technology. 2025;59:16452-16462. https://doi.org/10.1021/acs.est.5c06235
- [Google Scholar]
- Green sulfidated iron oxide nanocomposites for efficient removal of Malachite Green and Rhodamine B from aqueous solution. Water Science and Technology : A Journal of the International Association on Water Pollution Research. 2022;85:1202-1217. https://doi.org/10.2166/wst.2022.029
- [Google Scholar]
- Recovery of zinc resources from secondary zinc oxide via composite ammonia leaching: Analysis of Zn leaching behavior. Chemical Engineering Journal. 2023;472:144930. https://doi.org/10.1016/j.cej.2023.144930
- [Google Scholar]