Removal of Chromium(VI) from aqueous solution using guar gum–nano zinc oxide biocomposite adsorbent
Article History
-
Received: ,
Accepted: ,
Abstract
Guar gum–nano zinc oxide (GG/nZnO) biocomposite was used as an adsorbent for enhanced removal of Cr(VI) from aqueous solution. The maximum adsorption was achieved at 50 min contact time, 25 mg/L Cr(VI) conc., 1.0 g/L adsorbent dose and 7.0 pH. Langmuir, Freundlich, Dubinin–Kaganer–Radushkevich and Temkin isotherm models were used to interpret the experimental data. The data obeyed both Langmuir and Freundlich models (R2 = 0.99) indicating a multilayer adsorption of Cr(VI) onto the heterogeneous surface. The linear plots of Temkin isotherm showed adsorbent-adsorbate interactions. Moreover, the energy obtained from DKR isotherm (1.58–2.24 kJ/mol) indicated a physical adsorption of the metal ions onto the adsorbent surface, which implies more feasibility of the regeneration of the adsorbent. GG/nZnO biocomposite adsorbent showed an improved adsorption capacity for Cr(VI) (qm = 55.56 mg/g) as compared to other adsorbents reported in the literature. Adsorption process followed pseudo-second order kinetics; controlled by both liquid-film and intra-particle diffusion mechanisms. Thermodynamic parameters (ΔGo, ΔHo and ΔSo) reflected the feasibility, spontaneity and exothermic nature of adsorption. The results suggested that GG/nZnO biocomposite is economical, eco-friendly and capable to remove Cr(VI) from natural water resources.
Keywords
This article was originally published by Elsevier and was migrated to Scientific Scholar after the change of Publisher.
Peer review under responsibility of King Saud University.

1 Introduction
The contamination of water resources due to chromium(VI) is one of the serious environmental hazards. The industrial effluents from paints and pigments, and leather and chrome plating industries are major contamination sources. Generally, Cr(VI) exists as stable oxoanions in aqueous solution such as chromate ( ), hydrogen chromate ( ), dichromate ( ) and hydrogen dichromate ( ). The concentration of anionic species depends on solution pH and chromium concentration, which in turn affect its toxicity and bioavailability (Gaballah and Kilbertus, 1998). Cr(VI) toxicities include mutagenic (Cheng and Dixon, 1998), carcinogenic (Shumilla et al., 1999) and teratogenic (Asmatulla et al., 1998) effects. The permissible limit of Cr(VI) is 0.05 mg/L for potable water and 0.1 mg/L for discharge to inland surface water. Cr(VI) is reported to have damaging effects on the lungs, liver, nervous system and kidney in mammals. In view of its severe toxicity, the removal of Cr(VI) from water bodies is an important task. The conventional methods used for heavy metals removal from wastewater are precipitation, coagulation, chemical reduction, ion exchange and adsorption (Ali et al., 2012; Ali, 2010; Ali and Gupta, 2006). Most of these techniques are often expensive. However, the adsorption process is an attractive alternative due to its ease of operation, economic viability and effectiveness. Recently, adsorptive removal of Cr(VI) from wastewater using various adsorbents has been investigated by several workers (Ren et al., 2013; Ozer et al., 2012; Gupta et al., 2013; Shukla and Vankar, 2012; Annalisa et al., 2012; Rao et al., 2012; Borah et al., 2012; Khan and Singh, 2010; Rao and Rehman, 2010). It was observed that most of these adsorbents have limited applicability due to their low adsorption capacities, prolonged contact time and inability to work at natural pH of water. Therefore, it is imperative to develop more efficient and economical adsorbents with higher adsorption capacity, low contact time and ability to work at pH close to 7.
Guar gum is a polysaccharide composed of galactomannan units. Each unit of galactomannan consists of two units of β-d-mannopyranosyl joined via 1 → 4-linkage; with one unit of α-d-galactopyranosyl residue joined by 1 → 6-linkage as side chains. Hydrogel of guar gum has been used to remove Cu(II) in aqueous solution (Chauhan et al., 2009). Some workers (Yan et al., 2012; Singh et al., 2009a,b) modified guar gum with multi-walled carbon nanotubes, magnetic iron oxide nanoparticles, methyl-methycrylate, polyacrylamide or silica for the removal of toxic dyes (neutral red and methylene blue), Cr(VI) and Cd(II) from aqueous solution. It was observed that nano identities are also toxic to our environment; leading to chances of further environmental contamination (Ali, 2012) due mainly to difficulty in their separation. It was, therefore, considered worthwhile to incorporate nano ZnO particles with guar gum, which may be easily separated after adsorption process. In the present work, we report the adsorption efficiency of guar gum–nano zinc oxide (GG/nZnO) biocomposite, dynamics and thermodynamics of the uptake of Cr(VI) ions from aqueous solution.
2 Experimental
2.1 Reagents and chemicals
Guar gum (moisture content 5–6%) (CDH, India), zinc acetate (SRL, India), sodium hydroxide, potassium dichromate, potassium bromide, diphenylcarbazide (all Merck, India), isopropyl alcohol (IPA), absolute ethanol (S.D. Fine, India), sulfuric acid (Himedia, India) and nitric acid (Qualigens, India) were used as received.
2.2 Preparation of Cr(VI) solution
The stock solution of Cr(VI) (100 mg/L) was prepared by dissolving K2Cr2O7 in de-ionized water, which was diluted to desired concentrations (10 to 30 mg/L).
2.3 Preparation of adsorbent
Guar gum–nano zinc oxide (GG/nZnO) biocomposite was prepared by mixing 50 mg guar gum powder to 30 mL aqueous solution of isopropyl alcohol (3:1) in a 50 mL tri-necked round-bottom flask. The mixture was magnetically stirred at 60 °C to obtain a viscous gel. To this was added zinc acetate (100 mg) and the stirring continued till a homogeneous solution was obtained. NaOH solution (0.05 M) in isopropyl alcohol (10 mL) was then added to reduce zinc acetate to zinc oxide nanoparticles, which finally got immobilized within the polymeric guar mesh. The reaction mixture was centrifuged at 10,000 rpm for 10 min and washed with isopropyl alcohol to remove any free particles. It was subjected to lyophilization so as to obtain a dry powder of GG/nZnO biocomposite, which was stored in desiccators for adsorption studies.
2.4 Characterization of the adsorbent
The infrared spectra (4000–400 cm−1) of samples were recorded on a Perkin Elmer FT-IR BX2 instrument. The pellets were prepared by mixing 2 mg of the powdered sample with 200 mg of spectroscopic grade KBr. For TEM analysis, 5 mg of the dry nanoparticles were dispersed in 25 mL of ethanol in an ultra-sonicator. 10 mL of this nanoparticle dispersion was put on a formvar coated copper grid (1% solution of formvar in spectroscopic grade chloroform) and dried in vacuo. The dried grid was then examined under an electron microscope (Tem Technai 300KV, Ultra twin FEI with EDAX transmission electron microscope operating at 300 kV). Electron diffraction pattern of the zinc oxide and GG/nZnO biocomposite was also recorded. Scanning Electron Microscope (JEOL, model 3300) was used to investigate the surface morphology of ZnO nanoparticles and GG/nZnO biocomposite.
2.5 Adsorption studies
Adsorption experiments were carried out at a fixed agitation speed at room temperature (303 K) under batch mode technique. 10 mL of Cr(VI) ions solution of desired concentration (10–30 mg/L) was equilibrated with varying doses of GG/nZnO biocomposite (0.5–2 g/L) in a thermostatic water bath shaker for time intervals ranging from 10 to 60 min. The adsorbent was separated from the solution by centrifugation and the residual concentration of Cr(VI) ions in the supernatant liquid was determined spectrophotometrically following a standard procedure (Vogel, 1969) at 540 nm (λmax). For kinetic measurements, the experiments were performed using a fixed adsorbent dose with varying contact times at different Cr(VI) ion concentrations. The effect of varying solution pH on adsorption was studied in the range of 2–10. The solution pH was adjusted with dilute HCl or NaOH solution (both 0.01 M). The experiments were repeated three times and average values were taken. The amount of Cr(VI) ion adsorbed per unit mass of the adsorbent (qe, mg/g) was calculated using the following equation (Eq. (1)): (1) where, Co is the initial Cr(VI) concentration in mg/L before adsorption, Ce is equilibrium Cr(VI) concentration in mg/L after adsorption and m is the amount of adsorbent (g/L of metal ion solution). The percent adsorption was calculated from the relationship (Eq. (2)): (2)
3 Results and discussion
3.1 Characterization of the adsorbent
3.1.1 FTIR studies
FT-IR spectra of GG/nZnO biocomposite, guar gum and ZnO nanoparticles are given in Fig. 1. In the spectrum of guar gum, a band observed at 3400 cm−1 is ascribed to O–H stretching vibration while the band at 2925 cm−1 is due to C–H stretching of the –CH2 groups. The bands due to C–H bending and O–H bending appeared at 1458 and 1026 cm−1, respectively. The band at 871 cm−1 can be attributed to the C–H deformation mode. The band at 1654 cm−1 is due to the ring stretching of galactose and mannose. In addition, C–O–C and C–O stretching bands are observed, respectively, at 1155 and 1015 cm−1. The weak bands around 770 cm−1 are due to the ring stretching and ring deformation of α-d-(1–4) and α-d-(1–6) linkages. The formation of crystalline ZnO nanoparticles is confirmed from the characteristic peak at 470 cm−1 with a band at 3300 cm−1 due to some absorbed water on the ZnO surface. The decrease of the band related to hydroxyl groups in FTIR spectrum of GG/nZnO biocomposite indicated ZnO immobilized onto guar gum.
3.1.2 Transmission electron microscopic studies
TEM images of ZnO nanoparticles and GG/nZnO biocomposite [Fig. 2] showed that the nanoparticles are mono-dispersed and are spherical in shape. This confirmed that all the nuclei formed almost simultaneously and grew at the same rate. The result is in conformity with that of QELS [Fig. 2(c and d)], which showed no sign of agglomeration as the particles were uniform in shape and quite well dispersed.
3.1.3 Electron diffraction analysis
The electron diffraction patterns of ZnO nanoparticles and GG/nZnO biocomposite [Fig. 3] were studied. The fringe ring pattern clearly indicated the crystalline nature of the zinc oxide nanoparticles. The fused ring pattern revealed the amorphous nature of the GG/nZnO biocomposite.
3.1.4 Scanning electron microscopic studies
SEM images of ZnO nanoparticles [Fig. 4(a and b)] and GG/nZnO biocomposite [Fig. 4(c and d)] revealed the presence of ZnO nanoparticles immobilized onto guar gum.
4 Equilibrium adsorption studies
4.1 Effect of contact time
The effect of varying contact times on the percent removal and qe of Cr(VI) was studied at a constant adsorbent dose of 1 g/L GG/nZnO biocomposite and a concentration of 25 mg/L [Fig 5(a)]. It was observed that with the increase in contact time from 10 to 60 min., the qe and % removal increased till it reached equilibrium in 50 min., which was selected as the optimum contact time. The maximum percentage removal was 95.6%. The increased uptake of Cr(VI) ions with the passage of time might be due to the increased access of ions to active sites on the surface of adsorbent, resulting in an increase in the adsorption rate (Shen et al., 2009).
4.2 Effect of adsorbent dose
The percent uptake of Cr(VI) ions (25 mg/L) with varying dosages of GG/nZnO biocomposite is shown in Fig. 5(b). The percent removal increased with an increase in adsorbent dose and equilibrium was attained at an adsorbent dose of 1.0 g/L. The maximum percent removal at 1.0 g/L was 95.26%. No considerable increase in percent removal was seen thereafter. The increase in percent removal of adsorbate ions with increase in the adsorbent dose could be attributed to greater availability of adsorption sites. At equilibrium, the percent removal became constant probably because of the saturation of the available adsorption sites.
4.3 Effect of initial Cr(VI) concentration
The effect of varying initial Cr(VI) ion concentrations (10–30 mg/L) on the adsorption capacity of the adsorbent was studied at constant adsorbent dose and contact time [Fig. 5 (c)]. The percent removal increased with an increase in the initial concentration of Cr(VI) ion reaching equilibrium at 25 mg/L. The maximum amount adsorbed under these conditions was 95.62%.
4.4 Effect of pH
pH is an important factor controlling the adsorption process. The effect of pH on the adsorption efficiency of GG/nZnO biocomposite, in the pH range 2–10, is depicted in Fig. 5(d). The figure showed that percent removal of Cr(VI) increased with an increase in pH, with maximum adsorption occurring at pH 7. The percent removal steadily decreased thereafter. Similar variation in the adsorption of Cr(VI) with increase in pH has been reported by Rengaraj et al. (2003) and Bhattacharyya and Gupta (2006) with maximum adsorption occurring at pH 6 and 7, respectively. Cr(VI) exists in various oxoanionic forms in aqueous solution depending upon the solution pH. Below pH 1.0, the predominant species is H2CrO4. Between pH 1–6, Cr(VI) exists in the form of ( ), which dimerizes to with the release of a water molecule. Above pH 6, Cr(VI) exists in the form of . It has been suggested by Bhattacharyya and Gupta (2006) that at low pH the molecular form is predominantly adsorbed species, whereas at higher pH values the ionized form is preferentially adsorbed. The increase in adsorption up to pH 7 may be accounted on the basis of the fact that at low pH the species ( ) gets adsorbed as the adsorbent surface is positively charged.
The significance of using GG/nZnO biocomposite as an adsorbent lies in the fact that an optimum amount of adsorption of Cr(VI) was adsorbed at pH 7, which is the natural pH of about all natural water bodies.
4.5 Adsorption isotherms
The equilibrium data for adsorption of Cr(VI) onto GG/nZnO biocomposite were fitted into various isotherm models. The isotherm parameters and the regression coefficients (R2) corresponding to each model are given in Table 1.
| Isotherms | Isotherm constants | GG/nZnO biocomposite | ||
|---|---|---|---|---|
| 303 K | 308 K | 313 K | ||
| Langmuir | qm (mg/g) | 55.56 | 55.86 | 47.39 |
| b (L/mg) | 0.36 | 0.39 | 0.58 | |
| RL | 0.59 | 0.58 | 0.50 | |
| R2 | 0.99 | 0.99 | 0.99 | |
| Freundlich | nf | 1.39 | 1.39 | 1.54 |
| Kf (L/g) | 14.17 | 15.31 | 16.84 | |
| R2 | 0.99 | 0.99 | 0.99 | |
| DKR | qD (mg/g) | 27.48 | 27.72 | 27.22 |
| E (kJ/mol) | 1.58 | 1.58 | 2.24 | |
| R2 | 0.93 | 0.94 | 0.95 | |
| Temkin | Kt (L/g) | 3.53 | 3.92 | 5.16 |
| R2 | 0.97 | 0.97 | 0.98 | |
| b | 0.21 | 0.21 | 0.24 | |
4.5.1 Langmuir and Freundlich isotherm models
The linearized Langmuir and Freundlich adsorption isotherms are expressed as (Langmuir, 1918; Freundlich, 1906):
(3)
(4)
where qm (mg/g) is the maximum adsorption capacity to form a monolayer, b is the equilibrium constant, obtained from intercept and slope of Langmuir plot, respectively [Fig. 6(a)]. Kf (L/g) is related to adsorption capacity and nf is the exponent for favorable adsorption. Kf and nf were calculated from intercept and slope of Freundlich isotherm, respectively [Fig. 6(b)]. Langmuir adsorption isotherm assumes the occurrence of adsorption at a fixed number of definite localized sites with each site being homogenous and holding only one adsorbate molecule (monolayer) (Mckay et al., 1982). The Freundlich adsorption isotherm, on the other hand, assumes that adsorption occurs on a heterogeneous surface with the stronger binding sites occupied first and that the binding strength decreases with an increasing degree of site occupation. The R2 values for Langmuir and Freundlich isotherm models (Table 1) were closer to unity (0.99), which indicated that both Langmuir and Freundlich isotherm models were obeyed. This led to the conclusion that the adsorption of Cr(VI) onto the adsorbent was homogeneous and multilayer in nature.
It has been suggested that for favorable adsorption the values of the dimensionless separation factor, should be 0 < RL < 1. The value of RL represents whether adsorption is favorable (0 < RL < 1), unfavorable (RL > 1), linear (RL = 1) or irreversible (RL = 0). In the present study, the values of RL were 0.53–0.63 (Table 1); supporting a favorable adsorption process (Hall et al., 1966). At 303 K the adsorption capacity of the biocomposite was found to be 55.56 mg/g.
4.5.2 Temkin Isotherm model
This isotherm takes into account indirect adsorbate–adsorbent interactions on adsorbent surface. Temkin noted experimentally that heat of adsorption more often decreases with increasing coverage. Temkin adsorption isotherm is expressed as (Temkin and Pyzhev, 1940): (5) where, R is the gas constant, T is temperature in Kelvin, b is a constant related to the heat of adsorption and Kt is the equilibrium binding constant (L/g) corresponding to maximum binding energy. The linear plot of qe vs ln Ce at three different temperatures (303, 308 and 313 K) [Fig. 6(c)] for the adsorption system indicated the applicability of Temkin isotherm. The values of b and Kt were determined, respectively, from the slope and intercept of the plot (Table 1). Kt values at 303, 308, and 313 K were 3.53, 3.92, and 5.16 L/g, respectively; indicating considerable adsorbent-adsorbate interactions at all temperatures. The values of b at these three temperatures were 0.21, 0.21 and 0.24, respectively, indicating a small difference in heat of adsorption with change in temperature.
4.5.3 Dubinin–Kaganer–Radushkevich (DKR) isotherm model
DKR model is significant for calculating the apparent energy of adsorption, which predicts the type of adsorption i.e. physisorption or chemisorption. The model can be represented as (Dubinin and Radushkevich, 1947): (6) where is Polanyi Potential. The plot of ln qe vs yielded a straight line, thereby confirming the applicability of the model [Fig. 6(d)]. The magnitude of β was calculated from the slope of the plot which was used to calculate the magnitude of adsorption energy, . E values are useful in estimating the type of adsorption. The energy values in the range 1.0–8.0 and 8.0–16.0 kJ/mol indicate a physical and chemical adsorption, respectively. E values for the adsorption of Cr(VI) onto GG/nZnO biocomposite (1.58–2.24 kJ/mol) indicated a physical adsorption.
4.6 Adsorption dynamics
In order to predict the kinetics of adsorption and the rate controlling steps, Lagergren’s pseudo-first order, pseudo-second order, liquid-film and intra-particle diffusion models were studied. The values of different constants of these models are given in Table 2.
| Conc. | Pseudo-first order | Pseudo-second order | Liquid-film diffusion | Intra-particle diffusion | ||||||||
|---|---|---|---|---|---|---|---|---|---|---|---|---|
| (mg/L) | k1 (1/min) | qe (calc) (mg/g) | R2 | k2 (g/mg min) | qe (calc) (mg/g) | qe (exp) (mg/g) | R2 | Kf d × 10−2 (1/min) | R2 | Ki (mg min0.5/g) | Ci | R2 |
| 10 | 0.08 | 0.85 | 0.98 | 0.18 | 9.44 | 9.35 | 1.0 | 7.61 | 0.98 | 0.12 | 8.61 | 0.91 |
| 15 | 0.05 | 0.88 | 0.99 | 0.15 | 11.09 | 11.07 | 1.0 | 4.89 | 0.99 | 0.13 | 10.14 | 0.99 |
| 20 | 0.04 | 1.36 | 0.83 | 0.10 | 12.5 | 13.01 | 1.0 | 4.25 | 0.90 | 0.24 | 11.3 | 0.87 |
4.6.1 Lagergren’s pseudo-first order and pseudo-second order models
The experimental data were evaluated using Lagergren’s pseudo-first order (Lagergren, 1898) and pseudo-second order rate (Ho and McKay, 1999) equations:
(7)
(8)
where, qe and qt are the amount of Cr(VI) ions adsorbed per unit mass at equilibrium and at any time t, k1, and k2, are pseudo-first order and pseudo-second order rate constants, respectively. The kinetic parameters were calculated at different initial Cr(VI) concentrations from the intercept of the respective kinetic plots. The unity values of correlation coefficients for the pseudo-second order kinetic model [Fig. 7(a)] together with close agreement between calculated qe and experimental qe values (Table 2) suggested that pseudo-second order kinetic model best correlated the experimental data.
4.6.2 Intra-particle and liquid film diffusion models
The variation in the amount of adsorption with time at different initial Cr(VI) concentrations was analyzed for evaluating the role of diffusion in the adsorption process. Adsorption is considered to be a three step process. The first step involves transport of the adsorbate molecules from the aqueous phase to the film surrounding the adsorbent. In the second step diffusion of the solute molecules from the film to the adsorbent surface takes place. Finally, in the third step the adsorbate molecules diffuse into the pore interiors. The first step is bulk diffusion, the second is external mass transfer resistance and the third is intraparticle mass transfer resistance. When the intraparticle mass transfer resistance is the rate limiting step, then the adsorption process is described as being intraparticle diffusion controlled (Igwe and Abia, 2007). The intra-particle diffusion (Weber and Morris, 1964) and liquid film diffusion models (Boyd et al., 1949) are expressed as: (9) (10) where, ki (mg/g min0.5), Kfd (1/min), Ci and F(= qt/qe) are rate constants, boundary layer thickness and the fractional attainment of equilibrium at time t, respectively.
The plots of qt vs t0.5 and ln (1 − F) vs t [(Fig. 7(b and c)] for the adsorption system were linear. This indicated that both intraparticle diffusion and liquid film diffusion controlled the adsorption process. However, the plots did not pass through the origin. The deviation of liquid film diffusion plot from the origin may be attributed to the high speed of agitation used during kinetic experiments or may also be due to the difference between rate of mass transfer in the initial and final steps of adsorption (El-Ashtoukhy et al., 2008). The deviation of intraparticle diffusion plot from the origin indicated that the effect of external film resistance was not negligible.
4.7 Thermodynamic studies
The thermodynamic parameters are important to understand the energy and entropy changes during the adsorption process. The changes in enthalpy (ΔHo) and entropy (ΔSo) were determined from the slope and intercept, respectively of vant Hoff’s linear plots of log (qe/Ce) vs 1/T [Fig. 8] using the following equation:
(11)
The free energy change (ΔGo) was calculated using the following equation:
(12)

The calculated values are presented in Table 3.The positive values of ΔHo at different initial concentrations of Cr(VI) ions indicated the endothermic adsorption process. The magnitude of ΔHo being lower than 40 kJ/mol suggested physisorption of Cr(VI) onto GG/nZnO biocomposite (Bhatnagar et al., 2009). The positive ΔSo indicated an increased randomness at the solid-solution interface. The randomness might be attributed to the displaced water molecules gaining more translational entropy as compared to that lost by the metal ions during adsorption (Gopal and Elango, 2007). Gibbs’ free energy change (ΔGo) was negative indicating the adsorption process to be spontaneous in nature. The −ΔGo values increased with increasing temperature indicating thereby that adsorption was more favorable at a higher temperature.
| Conc. (mg/L) | ΔHo (kJ/mol) | ΔSo (kJ/mol K) | ΔGo (kJ/mol) | ||
|---|---|---|---|---|---|
| 303 K | K | K | |||
| 10 | 13.20 | 0.064 | 6.37 | 6.69 | 7.02 |
| 15 | 34.90 | 0.13 | 5.85 | 6.52 | 7.19 |
| 20 | 24.00 | 0.10 | 5.27 | 5.75 | 6.23 |
| 25 | 12.70 | 0.06 | 5.22 | 5.52 | 5.81 |
| 30 | 5.50 | 0.03 | 4.73 | 4.90 | 5.06 |
5 Evaluation of the adsorbent
Table 4 shows the comparison of the maximum adsorption capacities of various adsorbents for the removal of Cr(VI) from aqueous solution. The relatively higher adsorption capacity indicated that GG/nZnO is an efficient adsorbent for the removal of Cr(VI) from aqueous solution. Moreover, lesser contact time, lower adsorbent dosage, high percent removal, ability to work at pH 7 together with the bio-compatible and non-hazardous nature of the GG/nZnO biocomposite make this adsorbent more efficient and useful.
| Adsorbents | pH | Contact time (h) | Dose of adsorbent (g/L) | Isotherms | Kinetics | Thermodynamics | Adsorption capacity (mg/g) | References |
|---|---|---|---|---|---|---|---|---|
| Activated carbon-based iron- containing adsorbents | 2 | 48.00 | 0.6 | Langmuir, Freundlich | – | – | 68.49 | Liu et al.(2012) |
| GG/n ZnO biocomposite | 7 | 0.83 | 1 | Freundlich | Pseudo-second order, liquid film diffusion, intraparticle diffusion | Endothermic, spontaneous | 55.56 | This work |
| Hevea Brasilinesis sawdust activated carbon | 2 | 5 | 0.1 | Langmuir | Pseudo-second order, intraparticle diffusion | Endothermic, spontaneous | 44.05 | Karthikeyan et al.(2005) |
| Modified, cationic surfactant spent mushroom | 3.39 | 0.75 | 5 | Langmuir | Pseudo-first order | – | 43.86 | Jing et al. (2011) |
| Pine needles | 3 | 0.75 | 10 | Langmuir | – | – | 40.00 | Hadjmohammadi et al. (2011) |
| Eichhornia crassipes root biomass-derived activated carbon | 4.5 | 0.5 | 7 | Langmuir | Pseudo-second order | Endothermic, spontaneous | 36.34 | Giri et al. (2012) |
| Immobilized mycelia in carboxymethyl-cellulose (CMC)) of Lentinus sajor-caju | 2 | 2 | 25 | Langmuir, Freundlich | Pseudo-second order | – | 32.20 | Arıca and Bayramoglu (2005) |
| Aspergillus niger fungi | 3 | 12 | 0.2 | Freundlich | Pseudo-second order | Exothermic, spontaneous | 30.10 | Mungasavalli et al. (2007) |
| Poly- (methylacrylate) functionalized guar gum | 1 | 24 | 4 | Freundlich | Pseudo-second order | Exothermic, spontaneous | 29.67 | Singh et al. (2009a) |
| Terminalia arjuna nuts activated with zinc chloride | 1 | 10 | 2 | Langmuir, Freundlich | Pseudo-first order | – | 28.43 | Mohanty et al. (2005) |
| Oxidized activated carbon from peanut shell | 4 | 24 | 0.1 | Langmuir | Pseudo-first order, Pseudo-second order | Endothermic, spontaneous | 14.54 | AL-Othman et al. (2012) |
The larger adsorption capacity (55.56 mg/g) together with higher removal efficiency (98.63%) indicated that GG/nZnO is an efficient adsorbent for the removal of Cr(VI) from aqueous solution. Moreover, lower contact time (50 min.), adsorbent dose (1.0 g/L) and the ability to work at pH 7.0, which is close to pH of most water bodies suggested that it is a promising adsorbent as compared to most of other adsorbents.
6 Conclusions
The low contact time (50 min.) and adsorbent dose (1.0 g/L) together with high removal efficiency (98.63%) indicated that GG/nZnO biocomposite is a useful adsorbent for rapid and effective removal of Cr(VI) from aqueous solution. At pH 7, 98.63% Cr(VI) was removed with a contact time of 50 min. and an adsorbent dose 1.0 g/L. The maximum adsorption capacity calculated from Langmuir adsorption isotherm was found to be 55.56 mg/g at 303 K. The adsorption data best followed the Langmuir and Freundlich isotherm models. The pseudo-second order kinetic model described the data better than pseudo-first order, which is evident from the high correlation coefficient values and close agreement between experimental and calculated qe values. Thermodynamic parameters (ΔGo and ΔHo) suggested the adsorption process to be spontaneous and endothermic. Both liquid-film and intra-particle diffusions controlled the overall kinetics of the adsorption process. The developed adsorption system is inexpensive and advantageous for the removal of Cr(VI) from aqueous solution due to its small adsorption time, good adsorption capacity and ability to work at pH 7; a natural pH of most water bodies. This elucidates the practical applicability of the prepared adsorbent in the removal of Cr(VI) from natural water bodies.
Acknowledgment
One of the authors, Momina Nazir, is thankful to the University Grants Commission (UGC), New Delhi, India for financial assistance.
References
- The quest for active carbon adsorbent substitutes: inexpensive adsorbents for toxic metal ions removal from wastewater. Sep. Purif. Rev.. 2010;39:95-171.
- [Google Scholar]
- Advances in water treatment by adsorption technology. Nat. Lond.. 2006;1:2661-2667.
- [Google Scholar]
- Low cost adsorbents for removal of organic pollutants from wastewater. J. Environ. Manage.. 2012;113:170-183.
- [Google Scholar]
- Hexavalent chromium removal from aqueous medium by activated carbon prepared from peanut shell: adsorption kinetics, equilibrium and thermodynamic studies. Chem. Eng. J.. 2012;184:238-247.
- [Google Scholar]
- Study on the adsorption of chromium(VI) by hydrolyzed keratin/polyamide 6 blend nanofibres. J. Nanosci. Nanotechnol.. 2012;12:7250-7259.
- [Google Scholar]
- Cr(VI) biosorption from aqueous solutions using free and immobilized biomass of Lentinus sajor-caju: preparation and kinetic characterization. Colloids Surf., A. 2005;253:203-211.
- [Google Scholar]
- Hexavalent chromium-induced congenital abnormalities in chick embryos. J. Appl. Toxicol.. 1998;18:167-171.
- [Google Scholar]
- Removal of anionic dyes from water using Citrus limonum (lemon) peel: equilibrium studies and kinetic modeling. Sep. Sci. Technol.. 2009;44:316-334.
- [Google Scholar]
- Adsorption of chromium(VI) from water by clays. Ind. Eng. Chem. Res.. 2006;45:7232-7240.
- [Google Scholar]
- Preparation of ordered porous carbon from tea by chemical activation and its use in Cr(VI) adsorption. J. Porous Mat.. 2012;19:767-774.
- [Google Scholar]
- The exchange adsorption of ions from aqueous solution bioorganic zeolites II, Kinetics. J. Am. Chem. Soc.. 1949;69:2836-2842.
- [Google Scholar]
- Synthesis and characterization of novel guar gum hydrogels and their use as Cu2+ sorbents. Bioresour. Technol.. 2009;100:3599-3603.
- [Google Scholar]
- Analysis of repair and mutagenesis of chromium-induced DNA damage in yeast, mammalian cells, and transgenic mice. Environ. Health Perspect.. 1998;106:1027-1032.
- [Google Scholar]
- The equation of the characteristic curve of activated charcoal. Dokl. Akad. Nauk SSSR. 1947;55:327-329.
- [Google Scholar]
- Removal of lead(II) and copper(II) from aqueous solution using pomegranate peel as a new adsorbent. Desalination. 2008;223:162-173.
- [Google Scholar]
- Recovery of heavy metal ions through decontamination of synthetic solutions and industrial effluents using modified barks. J. Geochem. Explor.. 1998;62:241-286.
- [Google Scholar]
- Removal of Cr(VI) from aqueous solution by Eichhornia crassipes root biomass-derived activated carbon. Chem. Eng. J.. 2012;185–186:71-81.
- [Google Scholar]
- Kinetic and thermodynamic investigations of adsorption of fluoride onto activated aloe vera carbon. J. Indian Chem. Soc.. 2007;84:1114-1118.
- [Google Scholar]
- Chromium removal from water by activated carbon developed from waste rubber tires. Environ. Sci. Pollut. Res.. 2013;20:1261-1268.
- [Google Scholar]
- Removal of Cr(VI) from aqueous solution using pine needles powder as a biosorbent. J. Appl. Sci. Environ. Sanit.. 2011;6:1-13.
- [Google Scholar]
- Pore and solid-diffusion kinetics in fixed-bed adsorption under constant-pattern conditions. Ind. Eng. Chem. Fundam.. 1966;5:212-223.
- [Google Scholar]
- Adsorption kinetics and intraparticulate diffusivities for bioremediation of Co(II), Fe(II) and Cu(II) ions from waste water using modified and unmodified maize cob. Int. J. Phys. Sci.. 2007;2:119-127.
- [Google Scholar]
- Biosorption of Cr(VI) from simulated wastewater using a cationic surfactant modified spent mushroom. Desalination. 2011;269:120-127.
- [Google Scholar]
- Chromium(VI) adsorption from aqueous solution by Hevea Brasilinesis sawdust activated carbon. J. Hazard. Mater.. 2005;124:192-199.
- [Google Scholar]
- Removal of cadmium(II), lead(II) and chromium(VI) ions from aqueous solution using clay. Toxicol. Environ. Chem.. 2010;92:1435-1446.
- [Google Scholar]
- About the theory of so-called adsorption of soluble substances. K. Sven. Vetenskapsakademiens Handl.. 1898;24:1-39.
- [Google Scholar]
- The adsorption of gases on plane surfaces of glass, mica, and platinum. J. Am. Chem. Soc.. 1918;40:1361-1403.
- [Google Scholar]
- Preparation and evaluation of activated carbon-based iron-containing adsorbents for enhanced Cr(VI) removal: mechanism study. Chem. Eng. J.. 2012;189–190:295-302.
- [Google Scholar]
- Adsorption of dyes on chitin. I. Equilibrium studies. J. Appl. Polym. Sci.. 1982;27:3043-3057.
- [Google Scholar]
- Removal of chromium(VI) from dilute aqueous solutions by activated carbon developed from Terminalia arjuna nuts activated with zinc chloride. Chem. Eng. Sci.. 2005;60:3049-3059.
- [Google Scholar]
- Biosorption of chromium from aqueous solutions by pretreated Aspergillus niger: batch and column studies. Colloids Surf., A. 2007;301:214-223.
- [Google Scholar]
- Biosorption of Cr(VI) by free and immobilized Pediastrum boryanum biomass: equilibrium, kinetic, and thermodynamic studies. Environ. Sci. Pollut. Res.. 2012;19:2983-2993.
- [Google Scholar]
- Adsorption studies on fruits of Gular (Ficus glomerata): removal of Cr(VI) from synthetic wastewater. J. Hazard. Mater.. 2010;181:405-412.
- [Google Scholar]
- Removal of Cr(VI) from electroplating wastewater using fruit peel of Leechi (Litchi chinensis)Desal. Water Treat.. 2012;49:136-146.
- [Google Scholar]
- Synthesis of α-Fe2O3 nanofibers for applications in removal and recovery of Cr(VI) from wastewater. Environ. Sci. Pollut. Res.. 2013;20:155-162.
- [Google Scholar]
- Kinetics of removal of chromium from water and electronic process wastewater by ion exchange resins: 1200H, 1500H and IRN97H. J. Hazard. Mater. B. 2003;102:257-275.
- [Google Scholar]
- Preparation and application of magnetic Fe3O4 nanoparticles for wastewater purification. Sep. Purif. Technol.. 2009;68:312-319.
- [Google Scholar]
- Efficient biosorption of chromium(VI) ion by dry Araucaria leaves. Environ. Sci. Pollut. Res.. 2012;19:2321-2328.
- [Google Scholar]
- Chromium(VI) inhibits the transcriptional activity of nuclear factor-κB by decreasing the interaction of p65 with cAMP-responsive element-binding protein-binding protein. J. Biol. Chem.. 1999;274:36207-36212.
- [Google Scholar]
- Removal of chromium(VI) using poly (methylacrylate) functionalized guar gum. Bioresour. Technol.. 2009;100:1977-1982.
- [Google Scholar]
- Removal of cadmium from aqueous solutions by adsorption using poly(acrylamide) modified guar gum–silica nanocomposites. Sep. Purif. Technol.. 2009;67:251-261.
- [Google Scholar]
- Kinetic of ammonia synthesis on promoted iron catalyst. Acta Physiochim. USSR. 1940;12:327-356.
- [Google Scholar]
- Vogel, A.I., 1969. Textbook of Quantitative Inorganic Analysis, third ed. ELBS, p. 791.
- Advances in water pollution research. Oxford: Pergamon Press; 1964.
- Characterization of magnetic guar gum grafted carbon nanotubes and the adsorption of the dyes. Carbohydr. Polym.. 2012;87:1919-1924.
- [Google Scholar]