5.2
Impact Factor
Generic selectors
Exact matches only
Search in title
Search in content
Post Type Selectors
Search in posts
Search in pages
Filter by Categories
Corrigendum
Current Issue
Editorial
Erratum
Full Length Article
Full lenth article
Letter to Editor
Original Article
Research article
Retraction
Retraction notice
Review
Review Article
SPECIAL ISSUE: ENVIRONMENTAL CHEMISTRY
5.3
Impact Factor
Generic selectors
Exact matches only
Search in title
Search in content
Post Type Selectors
Search in posts
Search in pages
Filter by Categories
Corrigendum
Current Issue
Editorial
Erratum
Full Length Article
Full lenth article
Letter to Editor
Original Article
Research article
Retraction
Retraction notice
Review
Review Article
SPECIAL ISSUE: ENVIRONMENTAL CHEMISTRY
View/Download PDF
Original Article
2026
:19;
732026
doi:
10.25259/AJC_73_2026

Translate:

Synthesis and performance study of copolymer thickener for acid diversion

Author affiliations
College of Chemical Engineering, Sichuan University of Science & Engineering, Zigong, PR China
Oil & Gas Field Applied Chemistry Key Laboratory of Sichuan Province, Chengdu, PR China
Article History
Corresponding author(s)

* Corresponding authors: E-mail addresses: hytian0102@163.com (H. Tian), 59183228@qq.com (H. Quan)

Article tools · PDF & citations

Abstract

In response to the inadequate gel breaking performance of crosslinked acids during acid diversion in conventional oil and gas extraction, this paper presents the synthesis of a non-crosslinked copolymer thickener, which was synthesized from betaine monomer, acid-resistant monomer, cationic hydrophobic monomer, and acrylamide by aqueous solution polymerization. The synthesis conditions were optimized via the single-factor optimization method, and the molecular structure was characterized. Subsequently, the acid solubility, thickening ability, rheological properties of spent acid, and viscosity reduction performance of the thickener were systematically investigated. The results indicate that the synthesized thickener possesses excellent acid solubility and can dissolve in acid solutions rapidly. During the acid-rock reaction, the apparent viscosity of 0.6 wt% thickening acid increased from 18 mPa·s to 189 mPa·s, indicating that the thickener possesses excellent self-thickening capacity and can continuously thicken with the progression of the acid-rock reaction. Furthermore, the spent acid solution of the thickener shows favorable viscoelasticity, which is dominated by elasticity. Due to the non-crosslinking thickening mechanism of the thickener, no gel breaker is required, and water can directly reduce the viscosity of the spent acid to below 10 mPa·s. Moreover, additional studies have shown that adding an extremely small amount (0.3-0.4 wt%) of Tween 20 can reduce the viscosity of spent acid rapidly and effectively, significantly reducing the water consumption required for viscosity reduction solely by water. These findings provide a theoretical reference for the synthesis and application of non-crosslinking copolymer-based thickeners in oilfield acidizing operations.

Keywords

  • Acidizing
  • Non-crosslinked polymer
  • Rheological property
  • Self-thickening
  • Viscosity reduction
Licence
This is an open-access article distributed under the terms of the Creative Commons Attribution-Non Commercial-Share Alike 4.0 License, which allows others to remix, transform, and build upon the work non-commercially, as long as the author is credited and the new creations are licensed under the identical terms.

1. Introduction

In recent years, global consumption of oil and natural gas has been on the rise, while easily recoverable conventional resources are increasingly depleted, necessitating a shift in focus toward abundant unconventional oil and gas resources. These include coalbed methane, shale oil and gas, as well as other tight oil and gas resources [1,2]. Acidizing operations are one of the key technologies for mitigating reservoir damage and enhancing productivity [3]. However, conventional fracturing acidizing methods often fail to meet the requirements for efficient exploitation of unconventional oil and gas resources and struggle to improve reservoir production increment [4]. Additionally, due to the preferential flow of acid into high-permeability zones in traditional acidizing processes, low-permeability intervals are difficult to be effectively stimulated, resulting in the problem of non-uniform acid placement characterized by “over-acidization of high-permeability zones and neglect of low-permeability zones.” This defect not only reduces acidizing efficiency but may also exacerbate reservoir heterogeneity. To address these issues, acid diversion technology must be employed during acidizing operations to control the flow direction of acid, ensuring that the acid can effectively penetrate low-permeability reservoirs and thereby achieve uniform acid placement.

Classified by diversion mechanism, acid diversion technologies can be categorized into mechanical diversion and chemical diversion [5]. Due to the drawbacks of mechanical diversion, such as long construction time, difficulty in running tools downhole, high risk, high cost, and even unsatisfactory performance [6,7], chemical diversion has emerged as a more practical alternative. Extensive theoretical studies and model analyses by numerous researchers have confirmed that adding acid diverting agents during construction can redirect acid flow and generate new fractures [8,9].

Commonly used chemical acid diverting agents are mainly categorized into crosslinked polymer-based and viscoelastic surfactant (VES)-based types, which exhibit distinct effects on the temporary plugging mechanism of reservoirs and are both faced with certain challenges in practical applications. Crosslinked polymer diversion systems comprise crosslinkers, polymers, gel breakers, and other auxiliaries. Crosslinkers function to crosslink polymer chains, thereby forming a three-dimensional network structure with high viscosity, excellent shear resistance, and robust stability. While this system possesses favorable thickening and diverting capacity, it requires the addition of crosslinkers, leading to difficulties in complete gel breaking and flowback of acid during late-stage acidizing operations. Additionally, metal ions in crosslinkers can form precipitates in high-temperature or sulfur-bearing wells, causing secondary reservoir damage [10,11]. Liu et al. [12] pointed out in their study that in-situ crosslinked acids regulate polymer crosslinking via pH control, enabling gel formation within a specific pH range accompanied by a significant increase in viscosity. Nevertheless, the incorporation of crosslinking agents (e.g., Fe3+, Zr4+) inevitably contributes to formation damage following flowback. Du et al. [13] further emphasized that a major limitation of conventional polymer-based diverting acids is the residual polymer left in the formation after acid treatment. These prominent issues have emerged as technical bottlenecks that restrict the broader application of polymer-based diverting acids. The VES diverting acids offer advantages such as automatic thickening, in-situ diversion, spontaneous gel breakage, and relatively low formation damage. Muhammad Mansha et al. [14] synthesized three new zwitterionic gemini surfactants (1-3) and one known amide-sulfonated betaine surfactant (C18AMP3SB). In a 20 wt% CaCl2 solution at 90°C, the individual C18AMP3SB surfactant and its combination with the zwitterionic gemini surfactants (1-3) exhibited the best performance, with their apparent viscosities being 102, 14.6, 36.33, and 37.62 cPs, respectively. These systems have potential application value. However, they are associated with several limitations, including high required dosages, elevated application costs, and inadequate thermal stability under high-temperature conditions [15,16]. Liu et al. [17] reported that even oligomeric surfactants specifically designed for high-temperature reservoirs still necessitate a relatively high concentration (3-5 wt%), which substantially increases the cost per well treatment, thereby significantly hindering the large-scale deployment and practical application of these acid diverting systems.

Hydrophobically associating polymers exhibit excellent salt and acid resistance, and their unique hydrophobic association endows them with favorable thickening performance. Zheng and Huang [18] found that the hydrophobically associating polyacrylamide prepared by aqueous two-phase polymerization is able to form a three-dimensional network structure via intermolecular hydrophobic association, leading to a significant rise in the viscosity of the whole system. What’s more, inorganic salts can further boost its hydrophobic association effect, making the polymer retain high viscosity and superior viscoelasticity even in nearly saturated saline solutions. This polymer also shows good temperature resistance, with its viscosity retention rate remaining above 40% at 90°C, and its hydrophobic association characteristics grant it remarkable salt-tolerant thickening and shear resistance performance. Yang et al. [19] revealed that the content of hydrophobic groups plays a pivotal regulatory role in the associative thickening performance of betaine-type binary amphiphilic polymers. A higher hydrophobic group content can strengthen the intermolecular hydrophobic association and reduce the critical association concentration, while simultaneously enhancing the viscosity, viscoelasticity and thermal stability of polymer solutions. Besides, this category of polymer combines the anti-polyelectrolyte effect of betaine groups with the associative features of hydrophobic groups, thus exhibiting a distinctive salt-induced thickening characteristic. Its hydrodynamic radius expands in high-salt environments, allowing it to retain a good thickening effect under the conditions of high-salt reservoirs. These two studies both verify in terms of molecular structure and rheological properties that hydrophobic association is the fundamental mechanism underlying the superior salt resistance and thickening capabilities of hydrophobically associating polymers. Furthermore, the hydrophobic association effect can be further reinforced by optimizing polymerization approaches and conducting targeted modulation of molecular structures.

In this study, the non-crosslinked copolymer thickener TZXJ was synthesized through copolymerization of betaine monomer (CMB), acid-resistant monomer methacrylatoethyl trimethyl ammonium chloride (DMC), cationic hydrophobic monomer N, N-dimethyl octadecyl allyl ammonium chloride (C18DMAAC), and basic monomer acrylamide (AM). The synthesis conditions of thickener TZXJ were optimized, and its rheological properties and viscosity reduction performance were systematically evaluated.

2. Materials and Methods

2.1. Materials

Acrylamide (AM, AR), calcium carbonate powder (CaCO3, AR), were purchased from Chengdu Kelong Chemicals Co., Ltd. Methacrylatoethyl trimethyl ammonium chloride (DMC, 70 wt%), purchased from Chengdu Shundali Polymer Co., Ltd. N, N-dimethyl octadecyl allyl ammonium chloride (C18DMAAC, 70 wt%), purchased from Jiangsu Feixiang Chemical Group. 2,2’-azobis (2-methylpropionamidine) dihydrochloride (V50, 97 wt%), purchased from Shanghai Maclean Biochemical Technology Co., Ltd. High-temperature corrosion inhibitor (industrial grade), purchased from Chengdu Feierte Technology Development Co., Ltd. Betaine monomer (CMB), synthesized in the laboratory [20].

2.2. Synthetic route of thickener TZXJ

The thickener TZXJ was synthesized via free radical copolymerization of CMB, AM, DMC, and C18DMAAC, and its synthetic scheme is illustrated in Figure 1.

Synthesis route of thickener TZXJ.
Figure 1. Synthesis route of thickener TZXJ.

2.3. Synthesis method of thickener TZXJ

The dissolved CMB, acid-resistant monomer DMC, cationic hydrophobic monomer C18DMAAC, and basic monomer AM were introduced into a three-necked flask, which was subsequently immersed in a constant-temperature water bath (DZKW-S-6, Beijing Yongguangming Medical Instrument Co., Ltd.) and stirred uniformly. High-purity nitrogen gas was sparged through the solution for 30 min to remove the dissolved oxygen. The solution was then heated to the designated reaction temperature, and the initiator was added subsequently. After a defined reaction period, a gel-like product of the thickener was obtained. The resulting gel was cut into small pieces, dried in an electric blast drying oven (101-2A, Tianjin Taisite Instrument Co., Ltd.), and subsequently ground into a fine powder using a grinder to yield the powdered thickener TZXJ, which was stored in a desiccator for future use.

2.4. Evaluation method for thickener performance

The thickener and 1 wt% high-temperature corrosion inhibitor (based on the mass percentage of the 20 wt% HCl solution) were added to 480 g of 20 wt% HCl to prepare TZXJ thickening acid solutions (referred to as fresh thickening acid solutions) at a specific concentration. To simulate varying degrees of reaction between the acid solution and CaCO3, varying amounts of CaCO3 powder were introduced into separate batches of the fresh thickening acid solutions. Specifically, the amounts of CaCO3 were calculated based on the stoichiometric ratio in the acid-rock reaction equation, 32.88 g, 65.76 g, 98.64 g, and 121.65 g of CaCO3 were individually added to beakers containing the 20 wt% hydrochloric acid-based thickening acid solutions (fresh thickening acid solutions, 480 g), which can bring the hydrochloric acid concentration in the thickening acid after the reaction down from 20 wt% to 15 wt%, 10 wt%, 5 wt% and 1 wt%, respectively. The beakers were sealed with plastic wrap to minimize excessive volatilization of hydrochloric acid. After complete reaction in a water bath maintained at the designated temperature, thickening acid solutions with different extents of reaction (i.e., varying hydrochloric acid concentrations) were obtained. These reacted solutions were then transferred to the sample cup of a six-speed rotational viscometer (ZNN-D6B, Qingdao Tongchun Petroleum Instrument Co., Ltd.), and their apparent viscosities were measured at 100 rpm. Apparent viscosity of each sample was determined as three times the recorded reading, corresponding to a shear rate of 170 s-1.

2.5. Molecular structure characterization

After uniformly grinding purified thickener TZXJ with potassium bromide (KBr), a small amount of the finely ground powder was pressed into pellets for sample preparation. The molecular structure of the sample was characterized using a Fourier transform infrared spectrometer (FT-IR) (Nicolet iS5, Thermo Fisher Scientific Inc.). After fully dissolving the purified thickener TZXJ in deuterium oxide (D2O), the molecular structure of the sample was further characterized using a Nuclear magnetic resonance instrument (NMR) (Quantum-I Plus 600 MHz, Wuhan Zhongke Oxford spectroscopy technology Co., Ltd.).

Moreover, Gel permeation chromatography (GPC) was utilized to determine the number-average molecular weight (Mn), weight-average molecular weight (Mw), polydispersity index (PDI), and molecular weight distribution of the thickener TZXJ in this study. The measurements were conducted using a gel chromatograph (Alliance e2695, Waters Technology (Shanghai) Co., Ltd.). The test conditions are as follows: a PL aquagel-OH MIXED column is employed. A mixture of 0.2 mol/L NaNO3 and 0.01 mol/L NaH2PO4 is used as the mobile phase at a flow rate of 1 mL/min. PEG is adopted as the standard reference material.

2.6. Preparation of spent acid

Adding TZXJ to 20 wt% HCl solutions to prepare 0.8 wt% and 1.2 wt% TZXJ fresh thickening acid solutions at 30°C. Subsequently, CaCO3 powder was introduced into the freshly prepared acid solutions, and the reaction was allowed to proceed until the pH of the acid solutions reached 4-5, resulting in 0.8 wt% and 1.2 wt% thickened spent acids.

2.7. Rheological test of spent acid

Viscoelasticity is a fundamental rheological property, defined as the ability of a material to exhibit both elastic and viscous characteristics when subjected to deformation [21]. These dual behaviors are quantified by the storage modulus (G’) and the loss modulus (G’’), which represent the elastic and viscous responses of the material, respectively [22,23]. The overall viscoelastic behavior is described by the complex modulus (G*). And they satisfy Equations (1), (2) and (3).

(1) G*=σ/Γ

(2) G*=G'+iG"

(3) tanδ=G"/G'

In the formula:

σ—stress

Γ—strain

G* is a time-independent but frequency-dependent parameter. tanδ is the ratio of G’’ to G’, a larger tanδ value indicates fluid-like behavior or elastic damping characteristics (i.e., viscous behavior), whereas a lower tanδ value represents solid-like behavior (i.e., elastic behavior).

The viscoelastic properties of the TZXJ-thickened spent acid at 30°C were measured using a rotational rheometer (HAAKE MARS III, Thermo Fisher Scientific Inc.) at a test stress of 0.1 Pa. Additionally, the temperature resistance of the 1.2 wt% TZXJ-thickened spent acid was investigated at 120°C under a shear rate of 170 s-1 for 50 min.

3. Results and Discussion

3.1. Optimization of the synthesis conditions of thickener TZXJ

3.1.1. Effect of monomer ratio

With the total monomer concentration of AM, CMB, DMC, and C18DMAAC fixed at 20 wt%, initiator dosage maintained at 0.3 wt%, reaction temperature controlled at 50°C, reaction pH adjusted to 8, and reaction time set to 5 h, the thickener was synthesized by varying the monomer ratio of AM, CMB, DMC, and C18DMAAC. A 0.8 wt% thickening acid solution was prepared by incorporating thickener TZXJ and 1 wt% high-temperature corrosion inhibitor into 20 wt% hydrochloric acid. The apparent viscosity was measured with a six-speed rotational viscometer at 30°C. The effects of different monomer ratios on the thickening ability of the thickener are presented in Table 1.

Table 1. Effect of monomer ratio upon the thickening ability of the thickener.
No. Monomer ratio (AM:CMB:DMC: C18DMAAC) Apparent viscosity of acid solution (mPa·s)
0 g CaCO3 32.88 g CaCO3 65.76 g CaCO3 98.64 g CaCO3 121.65 g CaCO3
1 75.0:7.0:18.0:0.7 16.5 21.0 27.0 40.5 75.0
2 80.0:15.0:5.0:0.7 19.5 27.0 36.0 90.0 222.0
3 85.0:11.0:4.0:0.7 30.0 46.5 99.0 285.0 300.0
4 100.0:10.0:5.0:0.7 27.0 39.0 70.5 213.0 390.0
5 120.0:15.0:5.0:0.7 25.5 33.0 54.0 153.0 315.0
6 100.0:15.0:2.5:0.9 27.0 40.5 90.0 267.0 405.0
7 100.0:15.0:2.5:1.3 31.5 46.5 120.0 369.0 480.0

As shown in Table 1, during the transition from fresh thickening acid to spent acid, the apparent viscosity of the thickening acid progressively increases from a low to a high value. The monomer ratios significantly influence the apparent viscosity of the acid solution, with the contents of AM and CMB exhibiting a pronounced effect on the apparent viscosities of both the fresh and spent acid. The low viscosity of fresh acid promotes acid injection, while the high viscosity of spent acid is conducive to plugging high-permeability formations, driving subsequent acid to divert to low-permeability zones and thus achieving the acidizing of low-permeability formations [24]. Therefore, guided by the dual objectives of relatively low fresh acid viscosity while relatively high spent acid viscosity, and taking into comprehensive consideration the apparent viscosities of both acid states, the molar monomer ratio of AM:CMB:DMC: C18DMAAC at 100.0:15.0:2.5:0.9 yields relatively optimal performance, achieving apparent viscosities of 27.0 mPa·s for the fresh acid and 405.0 mPa·s for the spent acid. Consequently, this ratio is determined as the optimal molar ratio.

3.1.2. Effect of reaction pH

With the monomer concentration fixed at 20 wt%, initiator dosage maintained at 0.3 wt%, reaction temperature controlled at 50°C, reaction time set to 5 h, and the monomer ratio of AM, CMB, DMC, and C18DMAAC controlled at 100.0:15.0:2.5:0.9, thickener TZXJ was synthesized by varying the reaction pH. A 0.8 wt% thickening acid solution was prepared by incorporating thickener TZXJ and 1 wt% high-temperature corrosion inhibitor into 20 wt% HCl. The apparent viscosity was measured with a six-speed rotational viscometer at 30°C. The effects of different reaction pH values on the thickening ability of the thickener are presented in Table 2.

Table 2. Effect of reaction pH upon the thickening ability of thickener.
No. pH Apparent viscosity of acid solution (mPa·s)
0 g CaCO3 32.88 g CaCO3 65.76 g CaCO3 98.64 g CaCO3 121.65 g CaCO3
1 5 22.5 30.0 51.0 180.0 405.0
2 6 24.0 31.5 60.0 198.0 390.0
3 7 25.5 39.0 87.0 255.0 390.0
4 8 27.0 40.5 90.0 267.0 405.0
5 9 30.0 51.0 105.0 330.0 405.0

As shown in Table 2, the reaction pH values ranging from 5 to 9 have a relatively minor influence on the thickening ability of the thickener overall. Fresh thickening acid’s apparent viscosity rises steadily with increasing reaction pH. Adding 121.65 g of CaCO3 results in nearly unchanged apparent viscosity of the final spent acid, by comparison, a 98.64 g CaCO3 dosage leads to significant variations in the viscosity of thickening acids prepared under different pH conditions. The 0.8 wt% thickening acid demonstrates higher apparent viscosity (> 250 mPa·s) when applied in more concentrated acid environments, which can promote early diversion of subsequent acid fluids and thereby improve acidification efficiency in heterogeneous formations. Therefore, considering both the apparent viscosity of the fresh thickening acid and its increasing trend with pH, pH 7 is identified as the optimal reaction pH.

3.1.3. Effect of the dosage of initiator

With the monomer concentration fixed at 20 wt%, reaction temperature maintained at 50°C, reaction pH adjusted to 7, reaction time set to 5 h, and the ratio of AM, CMB, DMC, and C18DMAAC controlled at 100.0:15.0:2.5:0.9, the thickener was synthesized by varying the initiator dosage. A 0.8 wt% thickening acid solution was prepared by adding thickener TZXJ and 1 wt% high-temperature corrosion inhibitor to 20 wt% hydrochloric acid. The apparent viscosity was measured with a six-speed rotational viscometer at 30°C. The effects of different initiator dosages on the thickening ability of the thickener are presented in Table 3.

Table 3. Effect of the dosage of the initiator upon the thickening ability of the thickener.
No. Dosage of initiator (wt%) Apparent viscosity of acid solution (mPa·s)
0 g CaCO3 32.88 g CaCO3 65.76 g CaCO3 98.64 g CaCO3 121.65 g CaCO3
1 0.1 34.5 58.5 129.0 345.0 435.0
2 0.2 30.0 46.5 114.0 315.0 435.0
3 0.3 25.5 39.0 87.0 255.0 390.0
4 0.4 24.0 36.0 79.5 225.0 375.0
5 0.5 21.0 31.5 63.0 210.0 360.0

As shown in Table 3, the apparent viscosity of both fresh thickening acid and spent acid continuously decreased with increasing initiator dosage. This trend can be attributed to the fact that a lower initiator concentration generates fewer free radicals, which favors the formation of a thickener with a higher molecular weight. At lower initiator loadings, fewer free radicals form, resulting in thickeners with higher molecular weights and better thickening capacity, which translates to higher apparent viscosities for both fresh and spent acid. In contrast, higher initiator dosages generate more free radicals, raising the number of active sites and favoring chain transfer [25]. This yields thickeners with lower molecular weights, which in turn reduces the apparent viscosity of fresh acid and weakens thickening performance. As such, the molecular weight of the synthesized thickener needs to be controlled within a reasonable range: excessively high values hinder acid solubility, while overly low ones lead to poor thickening ability. Overall, the thickener prepared with a 0.3 wt% initiator dosage exhibits a relatively low apparent viscosity in fresh acid and a relatively high apparent viscosity in spent acid, making this initiator dosage the optimal one.

3.1.4. Effect of monomer concentration

With the initiator dosage maintained at 0.3 wt%, reaction temperature controlled at 50°C, reaction pH adjusted to 7, reaction time set to 5 h, and the ratio of AM, CMB, DMC, and C18DMAAC controlled at 100.0:15.0:2.5:0.9, the thickener was synthesized by varying the monomer concentration. A 0.8 wt% thickening acid solution was prepared by incorporating thickener TZXJ and 1 wt% high-temperature corrosion inhibitor into 20 wt% hydrochloric acid. The apparent viscosity was measured with a six-speed rotational viscometer at 30°C. The effects of different monomer concentrations on the thickening ability of the thickener are presented in Table 4.

Table 4. Effect of monomer concentration upon the thickening ability of the thickener.
No. Monomer concentration (wt%) Apparent viscosity of acid solution (mPa·s)
0 g CaCO3 32.88 g CaCO3 65.76 g CaCO3 98.64 g CaCO3 121.65 g CaCO3
1 15 16.5 24.0 34.5 87.0 240.0
2 20 25.5 39.0 87.0 255.0 390.0
3 25 27.0 45.0 99.0 306.0 405.0
4 30 30.0 49.5 117.0 345.0 375.0
5 35 31.5 60.0 156.0 360.0 390.0

As shown in Table 4, an increase in monomer concentration leads to a higher collision probability between monomers and free radicals, thereby promoting the degree of polymerization. Consequently, fresh thickening acid exhibits a continuous increase in apparent viscosity. Meanwhile, the acid reacted completely with 121.65 g of CaCO3 shows a steady viscosity rise with increasing monomer concentration. At a monomer concentration of 25 wt%, the spent acid from the polymerized thickening acid reaches its maximum apparent viscosity. When the monomer concentration exceeds 25 wt%, the excessively high monomer content will increase the risk of explosive polymerization during the polymerization process, which will reduce the performance of the thickener and the viscosity of the spent acid. Therefore, considering both the apparent viscosities of the fresh thickening acid and the spent acid, as well as the overall thickening performance, 25 wt% is determined to be the optimal monomer concentration.

Based on the optimization experimental results of the aforementioned factors, the optimal synthesis conditions were determined as follows: the molar ratio of AM, CMB, DMC, and C18DMAAC was 100.0:15.0:2.5:0.9; the initiator dosage was 0.3 wt%; the reaction temperature was 50 °C; the reaction pH was 7; the reaction time was 5 h; and the monomer concentration was 25 wt%.

3.2. Molecular structure characterization

The infrared spectrum and 1H NMR spectrum of TZXJ are presented in Figure 2. As shown in Figure 2, the absorption peaks at 3424 cm-1 and 1663 cm-1 are assigned to the stretching vibrations of the N–H and C=O groups in the polymer, respectively. The absorption peaks observed at 2928 cm-1 and 2853 cm-1 are attributed to the stretching vibrations of methyl (–CH3) and methylene (–CH2) groups within the polymer structure. Furthermore, the stretching vibration peak of the COO– groups appears at 1398 cm-1, while the absorption bands at 1202 cm-1 and 1129 cm-1 originate from the stretching vibrations of C–O groups in the polymer.

(a) The infrared spectrum and (b) 1H NMR spectrum of thickener TZXJ.
Figure 2. (a) The infrared spectrum and (b) 1H NMR spectrum of thickener TZXJ.

1H-NMR (600 MHz, D2O): δ = 0.90 (12, –CH3), δ = 1.20 (11, 18, 19, –(CH2)14–, –CH2–, –CH3), δ = 1.31 (10, 14, –CH2-, –CH3), δ = 1.64 (1, 4, 9, 13, –CH2–, –CH2–, –CH2–, –CH2–), δ = 2.20 (2, 5, 22, –CH–, –CH–, –CH2–), δ = 3.10 (6, –CH2–N), δ = 3.24 (7, 8, 21, 23, CH3–N–CH3, N–CH2–, N–CH2–, –CH2–N), δ = 3.65 (16, 17, 24, –CH2–N, N–(CH3)3, CH3–N–CH3), δ = 3.89 (25, N–CH2COO–,), δ = 4.53 (15, –O–CH2–). Based on the analysis of the infrared spectrum and 1H NMR spectrum, the obtained polymer is confirmed to possess the initially designed structure, indicating that the polymer (TZXJ) is consistent with the target product.

The results measured by the gel chromatograph show that Mn is 6.51×104, Mw is 3.68×105, and PDI (Mw/Mn) is 5.65. This indicates that the synthesized thickener TZXJ exhibits a relatively low molecular weight and a relatively high PDI. A relatively high PDI is mainly due to the characteristic of random copolymerization and notable differences in monomer reactivity. These differences give rise to unbalanced chain propagation rates during the copolymerization process, thus broadening the molecular weight distribution of the resulting products. Low molecular weight components allow the thickener to dissolve rapidly in a strongly acidic environment, whereas the relatively high molecular weight ones can boost the formation of a network structure during the acid-rock reaction. The smaller molecular weight of the thickener enables its rapid dissolution, and the thickening acid formed after dissolution exhibits a low initial viscosity, which facilitates acid fluid injection. Meanwhile, the viscosity of the spent acid after gel breaking is also low, which is beneficial for flowback.

3.3. Determination of acid dissolving time

TZXJ thickener powder was incorporated into a 20 wt% hydrochloric acid solution at a dosage of 0.8 wt%. The acid solution was then uniformly stirred at 30 °C using a constant-speed stirrer operating at 350 r/min. Under a shear rate kept consistently at 170 s-1, the acid solution’s apparent viscosity was recorded with a six-speed rotational viscometer every 5 min. A dissolution time curve of the thickener was generated by plotting the apparent viscosity of the acid solution as a function of time. The experimental results are presented in Figure 3.

Acid dissolving time of thickener TZXJ.
Figure 3. Acid dissolving time of thickener TZXJ.

It can be observed from Figure 3 that, as the stirring time increases, apparent viscosity of the 0.8 wt% thickening acid initially rises and subsequently stabilizes. This indicates that once the thickener is fully dissolved, the apparent viscosity of the acid solution reaches a steady state. According to the industry standard SY/T-6214-2016, thickeners for thickening acid require a dissolution time of less than 4h. In contrast, the acid dissolution time of this thickener is only 20 min, a remarkably short time reflecting its excellent solubility. This is because the thickener contains a high proportion of AM with strong acid solubility. Meanwhile, DMC, a quaternary ammonium cationic monomer with Cl-, also exhibits good solubility in hydrochloric acid. In addition, the content of the cationic hydrophobic long-chain monomer C18DMAAC is relatively low, which is conducive to the rapid dissolution of the thickener in hydrochloric acid.

3.4. Study on the thickening ability of thickener TZXJ under different dosages

Thickening acid solutions with varying dosages of thickener TZXJ were prepared by adding TZXJ to 20 wt% HCl solution. These solutions were maintained in a 30°C water bath, and different amounts of CaCO3 were added to each, the apparent viscosities were measured after the complete reaction between acid and CaCO3. The thickening properties of thickening acid solutions with different TZXJ concentrations are presented in Figure 4.

The TZXJ-thickened acid’s performance under different dosages.
Figure 4. The TZXJ-thickened acid’s performance under different dosages.

Figure 4 reveals that the apparent viscosity of the thickening acid solutions increases consistently with the rising mass of added CaCO3, and the thickener exhibits remarkable thickening performance as the acid-rock reaction proceeds continuously. This is attributed to the gradual increase in calcium chloride concentration in the acid solution during the acid-rock reaction, which continuously enhances the association of the hydrophobic chains of thickener TZXJ [11,26]. Meanwhile, the chelation between the betaine functional groups on the TZXJ molecular chains and Ca2+ is progressively strengthened [27], leading to a gradual rise in the strength of the associative network structure formed by TZXJ and thus endowing the thickener with excellent thickening properties. A higher dosage of the thickener results in a greater initial viscosity of the fresh acid, and the apparent viscosity of the acid solution after reacting with the same amount of CaCO3 increases accordingly. The initial viscosities of the thickened acids with 0.6 wt%, 0.8 wt%, 1.0 wt%, and 1.2 wt% dosages were 18 mPa·s, 39 mPa·s, 63 mPa·s, and 120 mPa·s, respectively. After adding 121.68 g of CaCO3, the apparent viscosities of the corresponding thickened spent acids reached 189 mPa·s, 285 mPa·s, 366 mPa·s, and 435 mPa·s, respectively. Notably, it can be seen that when 65.76 g of CaCO3 is added to react completely with the 1.2 wt% TZXJ thickening acid, its apparent viscosity reaches 315 mPa·s, exhibiting a relatively high apparent viscosity and thus possessing diversion capacity. At this stage, the acid concentration remains high (approximately 10 wt% HCl), indicating that the thickener possesses diversion capacity under high hydrochloric acid concentrations. The acid fluid already demonstrates excellent diversion capability without the need for complete reaction to the spent acid stage, consequently, this thickening acid is capable of diverting the subsequently injected acid fluids in advance.

Prevalent VES self-diverting acid systems remain at a relatively low viscosity during the initial and middle stages of acid-rock reactions (i.e., under high-concentration hydrochloric acid conditions), making it difficult to establish effective flow resistance [28]. A dramatic surge in the viscosity of spent acid occurs only in the late stage of the reaction, when the pH rises to 3.6-5 and the Ca2+ generated from the reaction reaches a critical concentration [29,30]. By contrast, the TZXJ thickener developed in this study enables continuous automatic thickening throughout the entire acid-rock reaction process, gradually increasing the acid viscosity from the initial reaction stage. This allows for the establishment of effective flow resistance at an earlier stage, facilitating the early diversion of subsequent acid fluids.

3.5. Study on the rheological properties of TZXJ-thickened spent acid

3.5.1. Constitutive equation of spent acid

The relationship between shear rate and shear stress of the TZXJ-thickened spent acid at 30°C was investigated using a rotational rheometer. The results are presented in Figure 5.

Relationship between shear rate and shear stress of TZXJ-thickened spent acid.
Figure 5. Relationship between shear rate and shear stress of TZXJ-thickened spent acid.

Curve regression analysis was conducted on the shear stress and shear rate data, enabling the derivation of the constitutive equation for TZXJ-thickened spent acid at 30°C. This equation serves as a model that characterizes their relationship.

(4) σ=15.74 γ 0.21  (R2 =0.88)

(5) σ=25.48 γ 0.18  (R2 =0.86)

In the formula:

σ—shear stress, Pa

γ—shear rate, s-1

The exponents in Equations (4) and (5) are both less than 1, indicating that the TZXJ-thickened spent acid exhibits shear-thinning behavior characteristic of pseudoplastic fluids. With relatively high consistency coefficients reflecting substantial viscosity, the rheological behavior of the TZXJ spent acid can be adequately described by the non-Newtonian power-law constitutive equation, expressed as σ = Kγⁿ (n < 1) [31,32].

The R2 values for the constitutive equation fits (0.86, 0.88) are relatively low. The specific reasons for the relatively low R2 are as follows: The test covers a wide shear rate range of 0-600 s-1, including the low shear rate region with dynamic structural rearrangement and the medium-high shear rate region with significant shear thinning behavior. The network structure formed by hydrophobic association in the system has a dynamic association-dissociation equilibrium under shear action. For the viscoelastic hydrophobic association thickening system, the rheological behavior varies significantly in different shear rate intervals, and it is difficult for a single constitutive model to achieve an extremely high fitting accuracy in the full shear rate range. Notably, the fitting parameters obtained from the power-law model have clear physical significance. The flow behavior index “n” of both systems is less than 1, which accurately characterizes the shear-thinning property of the thickened spent acid; the consistency coefficient K increases with the increase of thickener concentration, which is completely consistent with the change rule of the apparent viscosity of the system.

3.5.2. Study on the viscoelasticity and temperature resistance of spent acid

The results of viscoelasticity and high-temperature resistance of spent acid are presented in Figure 6.

Viscoelasticity (30°C) and high-temperature resistance (120°C) of TZXJ-thickened spent acid.
Figure 6. Viscoelasticity (30°C) and high-temperature resistance (120°C) of TZXJ-thickened spent acid.

As can be observed from Figure 6, which presents the complex modulus curves of the TZXJ-thickened spent acid solutions at 30°C, the complex modulus of the 1.2 wt% thickened spent acid is considerably higher than that of the 0.8 wt% thickened spent acid. Meanwhile, the complex modulus of the 0.8 wt% thickened spent acid increases with increasing oscillation frequency, whereas that of the 1.2 wt% thickened spent acid shows negligible variation. This suggests that the viscoelastic behavior of the 0.8 wt% thickened spent acid is slightly enhanced with increasing oscillation frequency, while the viscoelasticity of the 1.2 wt% thickened spent acid remains essentially unchanged. Furthermore, as illustrated in the tanδ curves of the thickened spent acid solutions at 30°C, the tanδ values for both the 0.8 wt% and 1.2 wt% thickened spent acids exhibit distinct variation trends across the oscillation frequency range. Notably, all tanδ values are less than 1, indicating that the spent acid is a viscoelastic fluid dominated by elasticity. This is because the TZXJ spent acid contains a high concentration of CaCl2, which enhances the association strength of the hydrophobic chains of TZXJ. Meanwhile, the betaine functional groups on the TZXJ molecular chains chelate with calcium ions, further reinforcing the associative network structure and thus endowing the TZXJ spent acid with excellent viscoelasticity [11,26,27]. The tanδ of the 0.8 wt% thickened spent acid slightly decreases first and then slowly increases with the rise in oscillation frequency, showing a minor overall fluctuation. Whereas the tanδ of 1.2 wt% thickened spent acid decreases significantly as the oscillation frequency increases. This indicates that the elasticity-dominated characteristic of t the 0.8 wt% thickened spent acid slightly strengthens first and then slowly weakens with the increase in scanning frequency, with an overall negligible change. In comparison, the elastic dominance of the 1.2 wt% thickened spent acid is markedly enhanced as the scanning frequency increases. The different variation trends of tanδ with oscillation frequency for the 0.8 wt% and 1.2 wt% thickened spent acids are mainly attributed to the differences in the association network density and structural stability of the system. At lower polymer concentration (0.8 wt%), the hydrophobic association strength is relatively low, resulting in a loosely connected transient network. Under increasing oscillation frequency, the polymer chains have insufficient time to reform association structures after deformation, leading to a more pronounced viscous response and a noticeable increase in tanδ. In contrast, at higher concentration (1.2 wt%), a denser three-dimensional transient network is formed due to enhanced hydrophobic association and stronger Ca2+ bridging interactions. This network structure can effectively store elastic energy even under high-frequency oscillation, resulting in a more stable or decreasing tanδ trend. Therefore, the distinct tanδ-frequency behaviors reflect the transition from a weakly associated dynamic network to a more compact and elastic association structure as polymer concentration increases.

As shown in Figure 6, the apparent viscosity of the thickened spent acid declined gradually during heating to the test temperature. This was caused by the continuous high temperature, which disrupted the spatial network structure formed by hydrophobic association. When the temperature reaches the test temperature, its apparent viscosity tends to be stable. After shearing at 120 °C for 50 min, the apparent viscosity of the 1.2 wt% thickened spent acid remained at around 125 mPa·s, demonstrating that the thickened spent acid possessed good temperature resistance.

3.6. Study on the viscosity reduction properties of TZXJ-thickened spent acid

3.6.1. Study on the viscosity reduction properties of spent acids by water

Since this thickener is a non-crosslinked polymeric thickener, no crosslinking agent is incorporated into the acid solution. The viscosity enhancement mechanism does not involve chemical crosslinking, such as the formation of covalent bonds with crosslinking agents; consequently, the spent acid exhibits a viscosity reduction upon contact with formation water. The effect of water dilution ratio on the apparent viscosity of the spent acid was evaluated at 30°C using a six-speed rotational viscometer, and the results are presented in Figure 7.

Effect of dilution ratio of water on apparent viscosity of thickened spent acid.
Figure 7. Effect of dilution ratio of water on apparent viscosity of thickened spent acid.

As can be observed from Figure 7, apparent viscosity of the thickened spent acids decreases continuously with increasing water dilution ratio. Meanwhile, due to its higher concentration, the 1.2 wt% thickened spent acid exhibits a greater initial viscosity. When diluted to the same extent, its apparent viscosity remains significantly higher than that of the 0.8 wt% thickened spent acid at low dilution ratios. As the dilution ratio increases progressively, however, the difference in apparent viscosity between the two concentrations gradually diminishes. Consequently, a larger volume of water is required to reduce the apparent viscosity of the 1.2 wt% thickened spent acid to below 10 mPa·s. Specifically, when water equivalent to 2.16 times the volume of the spent acid is added, the viscosity of the 0.8 wt% thickened spent acid drops below 10 mPa·s; in contrast, for the 1.2 wt% thickened spent acid, water addition equivalent to 3.92 times the volume of the spent acid is necessary to achieve the same viscosity reducing effect. This behavior can be attributed to the continuous decrease in the concentrations of both TZXJ and calcium salt with increasing dilution. As a result, the associative and chelating structures within the solution are progressively disrupted and diminished, while the three-dimensional polymeric network structure is increasingly broken down. This structural evolution is macroscopically manifested as a sustained decline in apparent viscosity.

3.6.2. Study on the viscosity reduction properties of spent acids by viscosity reducers

Surfactants exert a significant influence on polymers [33,34]. Investigations into how different surfactants affect the apparent viscosity of thickened spent acid were thus carried out to initially identify surfactant types with effective spent acid viscosity reduction. Subsequently, further screening for high-performance viscosity reducers from these types was conducted by considering solubility and other factors and evaluating viscosity reduction efficacy.

Due to the poor solubility of anionic surfactants in acid, the study focused on cationic, zwitterionic, and nonionic surfactants. Cetyl trimethyl ammonium bromide (CTAB), octadecanamide hydroxypropyl sulfobetaine (OPHSB), and octylphenol polyoxyethylene ether (OP-10) were selected, respectively. At 30°C, the effect of different concentrations of these three surfactants on the apparent viscosity of TZXJ-thickened spent acid was evaluated using a six-speed rotational viscometer, and the results are presented in Figure 8.

Effect of viscosity reducer on apparent viscosity of TZXJ-thickened spent acid: (a) CTAB, (b) OPHSB, (c) OP-10.
Figure 8. Effect of viscosity reducer on apparent viscosity of TZXJ-thickened spent acid: (a) CTAB, (b) OPHSB, (c) OP-10.

As can be observed from Figure 8, CTAB, OPHSB, and OP-10 exhibit distinct trends in their effects on 0.8 wt% spent acid’s apparent viscosity. For 0.8 wt% TZXJ-thickened spent acid, the apparent viscosity initially decreases slightly with increasing CTAB dosage, followed by a significant increase until reaching a stable value. In contrast, the influence of OPHSB on the 0.8 wt% spent acid’s apparent viscosity is characterized by minor initial fluctuations, after which a pronounced decrease occurs until stabilization is achieved. At a dosage of 2.4 wt% of the spent acid, the spent acid’s apparent viscosity with OPHSB remains 108 mPa·s, with a still high apparent viscosity at the stable stage. Whereas OP-10 exerts a significant and rapid viscosity reduction effect on the 0.8 wt% spent acid, leading to a substantial decrease in apparent viscosity followed by stabilization. At a dosage of 0.6 wt% of the spent acid, the spent acid’s apparent viscosity drops to 36 mPa·s, a relatively low value. Thus, the nonionic surfactant OP-10 exhibits superior viscosity reduction efficacy for 0.8 wt% thickened spent acid.

Preliminary experimental studies revealed that the nonionic surfactant OP-10 exerts favorable viscosity reduction efficacy on the apparent viscosity of thickened spent acid. Further screening and investigation were thus conducted on three nonionic surfactants, including OP-10, Tween 20, and Tween 80, by taking into account factors such as solubility, focusing on their effects on the 0.8 wt% and 1.2 wt% spent acids’ apparent viscosity. The influence of different dosages of these three surfactants on the 0.8 wt% and 1.2 wt% spent acids’ apparent viscosity was determined using a six-speed rotational viscometer at 30°C. The results are shown in Figure 9.

Effect of viscosity reducer on apparent viscosity of TZXJ-thickened spent acid: (a) OP-10, (b) Tween 20, (c) Tween 80.
Figure 9. Effect of viscosity reducer on apparent viscosity of TZXJ-thickened spent acid: (a) OP-10, (b) Tween 20, (c) Tween 80.

As can be observed from Figure 9, the apparent viscosity of TZXJ-thickened spent acid solutions exhibits a consistent trend of rapid initial decrease followed by stabilization with increasing dosages of OP-10, Tween 20, and Tween 80. Due to its higher initial apparent viscosity compared to the 0.8 wt% thickened spent acid, the 1.2 wt% TZXJ-thickened spent acid requires a greater dosage of viscosity reducer to reach a stable viscosity level. Specifically, when OP-10 is added at 0.6 wt% of the spent acid solution, 0.8 wt% spent acid’s apparent viscosity (36.0 mPa·s) essentially ceases to decrease. In contrast, for the 1.2 wt% thickened spent acid solution, apparent viscosity (75.0 mPa·s) essentially ceases to decrease upon addition of 1.2 wt% OP-10. At a dosage of 0.3 wt% of the spent acid, Tween 20 caused the 0.8 wt% spent acid’s apparent viscosity to level off at 31.5 mPa·s with no further decrease. At a dosage of 0.4 wt% of the spent acid, Tween 20 led to the 1.2 wt% thickened spent acid, leveling off at 66.0 mPa·s with no further reduction. For Tween 80, the apparent viscosity of the 0.8 wt% thickened spent acid leveled off at 40.5 mPa·s at a dosage of 0.4 wt% of the spent acid with no further drop, while that of the 1.2 wt% thickened spent acid leveled off at 90.0 mPa·s at a dosage of 0.8 wt% of the spent acid with no further decrease. It can be concluded that Tween 20 exerted the most pronounced viscosity reduction effect on the apparent viscosity of thickened spent acid, requiring the lowest optimal dosage and yielding the lowest stable apparent viscosity for the spent acid. Tween 20 was thus identified as the optimal viscosity reducer, with its optimal dosages for the viscosity reduction of 0.8 wt% and 1.2 wt% thickened spent acids being 0.3 wt% and 0.4 wt% of the spent acid, respectively.

3.6.3. Study on viscosity reduction time of spent acid under the action of viscosity reducer and synergistic viscosity reduction by water dilution

Viscosity reduction time is also a key factor influencing the viscosity-reducing performance of viscosity reducers. At the optimal dosage of Tween 20, the viscosity reduction time of thickened spent acid was investigated. Furthermore, after apparent viscosity of the TZXJ-thickened spent acid decreased to a stable level, the effectiveness of water dilution for further viscosity reduction was examined, with the results shown in Figure 10. The test procedure for determining viscosity reduction time was as follows: Tween 20, at the optimal dosage, was added to the TZXJ-thickened spent acid. The change in apparent viscosity over time was measured at a shear rate of 170 s-1 using a six-speed rotational viscometer at 30°C.

(a) Viscosity reduction time test of TZXJ-thickened spent acid under the optimal amount of Tween 20. (b) Effect of dilution ratio of water on apparent viscosity of thickened spent acid after viscosity reduction by Tween 20.
Figure 10. (a) Viscosity reduction time test of TZXJ-thickened spent acid under the optimal amount of Tween 20. (b) Effect of dilution ratio of water on apparent viscosity of thickened spent acid after viscosity reduction by Tween 20.

As can be observed from Figure 10, at 30°C, apparent viscosity of the 0.8 wt% thickened spent acid decreased and then tended to stabilize after shearing at 170 s-1 for 1 min following the addition of 0.3 wt% Tween 20. Similarly, when 0.4 wt% Tween 20 was added to the 1.2 wt% thickened spent acid solution, its apparent viscosity also decreased and then tended to stabilize under the same shear conditions. Therefore, Tween 20 enables rapid viscosity reduction of the thickened spent acid, achieving a low-viscosity state that facilitates efficient flowback. Furthermore, apparent viscosity of the thickened spent acid after treatment with Tween 20 decreases progressively with increasing water dilution ratio. Specifically, upon adding water equivalent to 0.87 times the volume of the spent acid, 0.8 wt% spent acid’s apparent viscosity drops below 10 mPa·s. Upon addition of water at 1.74 times the volume of the spent acid, the apparent viscosity of t the 1.2 wt% thickened spent acid also dropped to below 10 mPa·s. In comparison with the water consumption required to reduce the 0.8 wt% and 1.2 wt% spent acids’ apparent viscosity to below 10 mPa·s via direct water dilution without Tween 20, this water consumption was significantly reduced, accounting for only 40.28% and 44.39% of the respective values.

4. Conclusions

In this paper, a thickener TZXJ that thickens automatically with the acid-rock reaction was synthesized, and its acid solubility, rheological properties of the spent acid, and viscosity reduction performance of the spent acid were studied. The results demonstrate that TZXJ has excellent continuous thickening ability in hydrochloric acid systems, with the viscosity of 0.6 wt% and 1.0 wt% thickening acid solutions increasing from 18 and 63 mPa·s to around 189 and 366 mPa·s, respectively. Moreover, the TZXJ-thickened spent acid presents excellent viscoelasticity, acting as an elasticity-dominated viscoelastic fluid, and also possesses outstanding temperature resistance. The viscosity of 1.2 wt% thickened spent acid remains at approximately 125 mPa·s after 50 min of shearing at 120°C. Both water dilution and the screened optimal viscosity reducer, Tween 20, can effectively lower the viscosity of the spent acid, and pre-treatment with Tween 20 can reduce the water consumption for subsequent dilution by more than 55% compared with the direct water dilution method. The thickener is applicable to hydrochloric acid systems and reservoirs with temperatures above 120°C. This work provides technical support for the application of non-crosslinked polymer thickeners in the efficient acidizing treatment of heterogeneous low-permeability reservoirs. Future research will focus on developing non-crosslinked polymer diverting acids that can automatically thicken and reduce viscosity in response to acid-rock reactions.

Acknowledgement

This work was supported by the Sichuan Science and Technology Program (2025ZNSFSC1351), by the Opening Project of Oil & Gas Field Applied Chemistry Key Laboratory of Sichuan Province (YQKF202210).

CRediT authorship contribution statement

Haiyang Tian: Conceptualization, methodology, investigation, funding acquisition, project administration, supervision, writing-review & editing, resources, data curation. Wenhua Zhou: Validation, investigation, visualization, writing-original draft, data curation, formal analysis. Hongping Quan: Resources, software. Zhiyu Huang: Software, resources.

Declaration of competing interest

There are no conflicts of interest.

Declaration of generative AI and AI-assisted technologies in the writing process

The authors confirm that there was no use of artificial intelligence (AI)-assisted technology for assisting in the writing or editing of the manuscript and no images were manipulated using AI.

References

  1. , , , , , , , . Distribution and potential of global oil and gas resources. Petroleum Exploration and Development. 2018;45:779-789. https://doi.org/10.1016/s1876-3804(18)30081-8
    [Google Scholar]
  2. . Unconventional energy resources: 2017 review. Natural Resources Research. 2019;28:1661-1751. https://doi.org/10.1007/s11053-018-9432-1
    [Google Scholar]
  3. , , , , , . Experimental study on solid acid systems for acid fracturing in ultrahigh-temperature carbonate reservoirs. ACS Omega. 2025;10:45309-45322. https://doi.org/10.1021/acsomega.5c04835
    [Google Scholar]
  4. , , , , , , . Experimental study on plugging performance and diverted fracture geometry during different temporary plugging and diverting fracturing in Jimusar shale. Journal of Petroleum Science and Engineering. 2022;215:110580. https://doi.org/10.1016/j.petrol.2022.110580
    [Google Scholar]
  5. , , , , , . Research and application progress of temporary plugging agent for acidification fracturing: A review. Geoenergy Science and Engineering. 2025;247:213600. https://doi.org/10.1016/j.geoen.2024.213600
    [Google Scholar]
  6. , , , , . Development and field application of strongly resilient temporary plugging diversion agent for fracturing. Journal of Petroleum Exploration and Production Technology. 2024;14:2073-2088. https://doi.org/10.1007/s13202-024-01814-7
    [Google Scholar]
  7. Chen, J., Wang, Y., Zhao X., Tang C., Gao Y., Zhou D., Zeng B., Liu X., Li W., Wu J., 2020. Chemical agents diversion with microseismic monitoring-new prospects of refracturing for open-hole horizontal well in tight oil reservoir of junggar basin, China. SPE/IATMI Asia Pacific oil gas conference and exhibition, October 29-31, 2019, Bali, Indonesia, paper No. SPE-196505-MS. https://doi.org/10.2118/196505-MS.
  8. , , , , , , , , . Research of a self-adaptive high-performance re-fracturing technology with knot temporary plugging in a thin reservoir with high stress. Chemistry and Technology of Fuels and Oils. 2023;58:1027-1034. https://doi.org/10.1007/s10553-023-01485-w
    [Google Scholar]
  9. , , , , , . Effects of saturated fluids on petrophysical properties of hot dry rock at high temperatures: An experimental study. Geothermics. 2024;121:103048. https://doi.org/10.1016/j.geothermics.2024.103048
    [Google Scholar]
  10. , , , , , , , . Synthesis and performance study of self-degradable gel plugging agents suitable for medium- and low-temperature reservoirs. ACS Omega. 2024;9:33702-33709. https://doi.org/10.1021/acsomega.4c02410
    [Google Scholar]
  11. , , , , , , , , . Two-level self-thickening mechanism of a novel acid thickener with a hydrophobic-associated structure during high-temperature acidification processes. Polymers. 2024;16:679. https://doi.org/10.3390/polym16050679
    [Google Scholar]
  12. , , , , , . Analysis and simulation of rheological behavior and diverting mechanism of in situ self-diverting acid. Journal of Petroleum Science and Engineering. 2015;132:39-52. https://doi.org/10.1016/j.petrol.2015.04.042
    [Google Scholar]
  13. , , , , . Influencing factors of viscoelastic surfactant diverting acid: A review. Petroleum Science and Technology. 2025;43:3270-3302. https://doi.org/10.1080/10916466.2024.2415521
    [Google Scholar]
  14. , , , . Synthesis, characterization, and viscosification of amidosulfobutaine and zwitterionic gemini surfactants. Journal of Surfactants and Detergents. 2021;24:697-706. https://doi.org/10.1002/jsde.12474
    [Google Scholar]
  15. , , , , , , . An innovative concept on deep carbonate reservoir stimulation: Three-dimensional acid fracturing technology. Natural Gas Industry B. 2020;7:484-497. https://doi.org/10.1016/j.ngib.2020.09.006
    [Google Scholar]
  16. Then, Y. L., Ling K. T., Goh S. H., Melice D. T., 2023. Evaluation and optimization of a novel high-density and high-temperature resistance VES-based fracturing fluid. Gas oil technology showcase and conference, March 13-15, 2023, Dubai, UAE, Paper No. SPE-214203-MS. https://doi.org/10.2118/214203-MS.
  17. , , , , , . Review on high-temperature-resistant viscoelastic surfactant fracturing fluids: state-of-the-art and perspectives. Energy & Fuels. 2023;37:9790-9821. https://doi.org/10.1021/acs.energyfuels.3c00488
    [Google Scholar]
  18. , . Self-assembly and regulation of hydrophobic associating polyacrylamide with excellent solubility prepared by aqueous two-phase polymerization. Colloids and Surfaces A: Physicochemical and Engineering Aspects. 2018;555:621-629. https://doi.org/10.1016/j.colsurfa.2018.07.048
    [Google Scholar]
  19. , , , , , , , , , , . Effect of hydrophobic group content on the properties of betaine-type binary amphiphilic polymer. Journal of Molecular Liquids. 2020;311:113358. https://doi.org/10.1016/j.molliq.2020.113358
    [Google Scholar]
  20. , , , , . Water-soluble ampholytic grafted polysaccharides. 1. Grafting of the zwitterionic monomer 2-(2-Methacrylo-Ethyldimethylammonio) ethanoate onto hydroxyethyl cellulose. Journal of Macromolecular Science, Part A. 2000;37:1247-1260. https://doi.org/10.1081/ma-100101152
    [Google Scholar]
  21. , , , , . Rheological considerations of pharmaceutical formulations: Focus on viscoelasticity. Gels (Basel, Switzerland). 2023;9:469. https://doi.org/10.3390/gels9060469
    [Google Scholar]
  22. , , , , . Universal relationship between linear viscoelasticity and nonlinear yielding in soft materials. Physical Review Letters. 2025;134:208202. https://doi.org/10.1103/PhysRevLett.134.208202
    [Google Scholar]
  23. , , . Direct computations of viscoelastic moduli of biomolecular condensates. The Journal of Chemical Physics. 2024;161:095103. https://doi.org/10.1063/5.0223001
    [Google Scholar]
  24. , , , , , , . Experimental study on the diversion characteristic of a viscous fluid in a heterogeneous reservoir. ACS Omega. 2022;7:46475-46485. https://doi.org/10.1021/acsomega.2c05278
    [Google Scholar]
  25. , , , , , . Efficient approach to produce functional polypropylene via solvent assisted solid-phase free radical grafting of multi-monomers. Applied Petrochemical Research. 2021;11:99-111. https://doi.org/10.1007/s13203-020-00261-9
    [Google Scholar]
  26. , , , , , . Hydrophobically modified polymer–surfactant self-assembly system: A study of a self-thickening diverting acid solution. ACS Omega. 2025;10:59021-59033. https://doi.org/10.1021/acsomega.5c07911
    [Google Scholar]
  27. , , , . Salt stimulus response of a carboxyl betaine amphoteric hydrophobic associative polyacrylamide. Russian Journal of Applied Chemistry. 2017;90:1193-1201. https://doi.org/10.1134/s1070427217070266
    [Google Scholar]
  28. , , , , , , , . Numerical simulation: Diverting study and analysis on nanoparticle-viscoelastic-surfactant acid in high-temperature carbonate reservoir. Physics of Fluids. 2024;36:076627. https://doi.org/10.1063/5.0220673
    [Google Scholar]
  29. , , . Numerical investigation of acid diversion using viscoelastic surfactant (VES) under single and two-phase flow conditions. Journal of Petroleum Exploration and Production Technology. 2025;15:37. https://doi.org/10.1007/s13202-025-01926-8
    [Google Scholar]
  30. Mou, J., Cai X., Liu M., Zhang Y., Zhang S., 2013. The mechanism of leakoff reduction of clean self-diversion acid in acid fracturing. IPTC 2013: International petroleum technology conference, March 26-28, 2013, Beijing, China, Paper No. cp-350-00223. https://doi.org/10.3997/2214-4609-pdb.350.iptc16720.
  31. , , , . Numerical simulation of droplet formation for non-newtonian power-law fluids in flow-focusing microchannels by lattice Boltzmann method. Chemical Engineering Journal. 2025;524:169161. https://doi.org/10.1016/j.cej.2025.169161
    [Google Scholar]
  32. , , , . Rheological property and thermodynamic parameters of Ficus carica Linn. pectin: A natural low-methoxyl pectin (LMP) with excellent pseudoplasticity. Food Chemistry. 2025;484:144317. https://doi.org/10.1016/j.foodchem.2025.144317
    [Google Scholar]
  33. , , , . Revealing the formation dynamics of janus polymer particles: Insights from experiments and molecular dynamics. Journal of Chemical Information and Modeling. 2023;63:7453-7463. https://doi.org/10.1021/acs.jcim.3c01547
    [Google Scholar]
  34. , . Steady shear rheology and surface activity of polymer-surfactant mixtures. Polymers. 2025;17:364. https://doi.org/10.3390/polym17030364
    [Google Scholar]
Show Sections